CHEMVEN

Photocatalytic Degradation of a Dye by TiO2

To demonstrate heterogeneous photocatalysis: TiO2 nanoparticles degrading methylene blue under UV/visible light.

Level: UniversitySafety: Needs supervisionTime: 2 h
Aim of Experiment: To demonstrate heterogeneous photocatalysis: TiO2 nanoparticles degrading methylene blue under UV/visible light.

Theoretical Foundations

TiO2 absorbs photons with energy above its band gap (3.2 eV), creating electron-hole pairs. Holes oxidise water to OH· radicals that mineralise dyes. The dye's absorbance decays with first-order kinetics only when light AND TiO2 are both present.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Beakers
  • UV lamp or bright sunlight
  • Magnetic stirrer
  • Colorimeter
  • Filter paper
  • Foil

Chemical Reagents

  • Titanium dioxide (anatase nanopowder)
  • Methylene blue (10 mg/L)
  • Distilled water

Step-by-Step Practical Procedure

  1. Prepare 100 mL of 10 mg/L methylene blue; add 0.10 g TiO2.
  2. Stir 15 min in the dark (adsorption equilibrium).
  3. Irradiate with stirring; withdraw filtered aliquots every 10 min.
  4. Measure absorbance at 665 nm.
  5. Run controls: light without TiO2; TiO2 in dark.
  6. Plot ln(A0/At) vs t; compare rate constants.

Observations & Expected Results

With light + TiO2 the blue fades markedly in 60 min (k ~ 0.02 min^-1); controls barely change - proving photocatalysis.

Worked Stoichiometric Calculations

Problem: Absorbance falls from 1.20 to 0.36 in 60 min. Find k and the half-life.

Working: k = (1/60)·ln(1.20/0.36) = (1/60)·ln(3.333) = (1/60)(1.204) = 0.0201 min^-1. t1/2 = 0.693/0.0201 = 34.5 min.

Safety Precautions & Hazard Control

  • UV lamp: wear UV goggles, avoid skin exposure.
  • Do not inhale TiO2 nanopowder - weigh carefully.
  • Filter aliquots before photometry (TiO2 scatters).

Waste Disposal Protocol

Recover TiO2 by filtration; dye filtrate to coloured waste.

Viva Voce Oral Defense Questions & Answers

Q: What are the roles of the electron and hole?

A: Holes oxidise H2O/OH^- to OH· radicals; electrons reduce O2 to superoxide - both degrade organics.

Q: Why is the dark-adsorption step needed?

A: To separate true photocatalytic loss from mere adsorption of dye on TiO2.

Q: Name a real-world application.

A: Self-cleaning glass, anti-pollution building coatings, and wastewater treatment.

← Back to Experiments Directory