Gels: Preparation of Silica Gel and Study of Thixotropy
To prepare silica gel and demonstrate thixotropy (shear-thinning with time-dependent recovery).
Theoretical Foundations
Acidifying sodium silicate gives silicic acid, which polymerises into a 3D network trapping water - a gel. Thixotropic gels (e.g. bentonite, some silica gels) liquefy on shaking and re-gel on standing, as weak interparticle bonds break and reform.
Required Apparatus & Chemicals
Laboratory Apparatus
- Beakers
- Glass rod
- Test tubes
- pH paper
Chemical Reagents
- Sodium silicate solution (water glass)
- Hydrochloric acid (2 M)
- Bentonite clay (for thixotropy demo)
- Distilled water
Step-by-Step Practical Procedure
- Mix 20 mL sodium silicate with 60 mL water.
- Add 2 M HCl slowly with stirring until pH ~7.
- Let stand - note gelation (tube inversion test).
- Prepare a bentonite suspension (5%); let it gel.
- Shake vigorously - it flows; let stand - it re-gels.
- Time the re-gelation.
Observations & Expected Results
Silica sets to a firm clear gel in minutes; bentonite liquefies on shaking and re-gels in ~2-5 min - reversible thixotropy.
Worked Stoichiometric Calculations
Problem: 20 mL of sodium silicate solution (density 1.4 g/mL, 30% Na2SiO3, M = 122.1) is used. What mass of SiO2 network forms (M_SiO2 = 60.1)?
Working: Mass silicate = 20 x 1.4 x 0.30 = 8.4 g = 0.0688 mol. SiO2 formed = 0.0688 x 60.1 = 4.14 g of silica network (hydrated).
Safety Precautions & Hazard Control
- Add acid slowly - local excess gives grainy gel.
- HCl is corrosive; wear gloves.
- Do not disturb the gel while it sets.
Waste Disposal Protocol
Silica gel to solid waste; bentonite to drain with water.
Viva Voce Oral Defense Questions & Answers
Q: What is a gel?
A: A semi-solid colloidal system with a continuous solid network trapping liquid.
Q: What is thixotropy?
A: Time-dependent shear thinning: the gel flows when shaken and rebuilds its structure on standing.
Q: Give two practical thixotropic materials.
A: Certain paints (non-drip) and drilling muds.