CHEMVEN

Polymer Molecular Mass from Intrinsic Viscosity (Mark-Houwink)

To determine the viscosity-average molecular mass of poly(vinyl alcohol) from its intrinsic viscosity.

Level: UniversitySafety: SafeTime: 2 h
Aim of Experiment: To determine the viscosity-average molecular mass of poly(vinyl alcohol) from its intrinsic viscosity.

Theoretical Foundations

For dilute polymer solutions, reduced viscosity extrapolated to zero concentration gives intrinsic viscosity [eta], related to molecular mass by the Mark-Houwink equation [eta] = K·M^a. Measuring flow times at several concentrations yields [eta] and hence M.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Ostwald viscometer
  • Thermostat at 25 C
  • Analytical balance
  • Volumetric flasks
  • Stopwatch
  • Pipettes

Chemical Reagents

  • Poly(vinyl alcohol) (PVA)
  • Distilled water
  • Acetone (cleaning)

Step-by-Step Practical Procedure

  1. Dissolve PVA in warm water to make 1.0 g/dL stock; prepare 0.8, 0.6, 0.4, 0.2 g/dL dilutions.
  2. Thermostat the viscometer at 25.0 C.
  3. Measure flow times of solvent (t0) and each solution (t).
  4. Compute eta_sp = (t - t0)/t0 and eta_red = eta_sp/c.
  5. Plot eta_red vs c; extrapolate to c = 0 to get [eta].
  6. Calculate M = ([eta]/K)^(1/a) using K = 6.3 x 10^-4 dL/g, a = 0.72.

Observations & Expected Results

eta_red rises linearly with c (Huggins plot); typical student [eta] ~ 1.2 dL/g giving M ~ 3.6 x 10^4 g/mol.

Worked Stoichiometric Calculations

Problem: Extrapolation gives [eta] = 1.20 dL/g. With K = 6.3 x 10^-4 dL/g and a = 0.72, find the viscosity-average molecular mass.

Working: M = (1.20/6.3 x 10^-4)^(1/0.72) = (1904.8)^1.3889. log10(1904.8) = 3.2799; 3.2799 x 1.3889 = 4.5555; M = 10^4.5555 = 3.6 x 10^4 g/mol.

Safety Precautions & Hazard Control

  • Dissolve PVA completely - undissolved gel gives false high times.
  • Filter solutions through a coarse filter.
  • Keep concentration low enough that chains do not entangle.
  • Strict temperature control.

Waste Disposal Protocol

Dilute polymer solutions to drain with water; acetone to organic waste.

Viva Voce Oral Defense Questions & Answers

Q: What is intrinsic viscosity physically?

A: The hydrodynamic volume per unit mass of an isolated polymer coil - a measure of chain size.

Q: What does the exponent a tell you?

A: a ~ 0.5 means a compact coil in a poor solvent; a ~ 0.8 means an extended chain in a good solvent.

Q: Why extrapolate to zero concentration?

A: To remove chain-chain interactions so [eta] reflects single isolated molecules.

← Back to Experiments Directory