CHEMVEN

Monolayer Coverage: Adsorption of Methylene Blue on Charcoal

To determine the monolayer adsorption capacity of charcoal for methylene blue and estimate its specific surface area.

Level: UniversitySafety: SafeTime: 90 min
Aim of Experiment: To determine the monolayer adsorption capacity of charcoal for methylene blue and estimate its specific surface area.

Theoretical Foundations

Large dye molecules like methylene blue form a monolayer on carbon surfaces; each molecule occupies a known area (~130 A^2). From the plateau adsorption (a_max) the surface area follows: A = (a_max/M)·N_A·sigma, a simple route to surface-area estimation without BET apparatus.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Stoppered flasks
  • Balance
  • Colorimeter or visual comparison tubes
  • Filtration set
  • Measuring cylinders
  • Volumetric flasks

Chemical Reagents

  • Methylene blue (0.01 M stock)
  • Activated charcoal (fine)
  • Distilled water

Step-by-Step Practical Procedure

  1. Prepare 50 mL of methylene blue solutions: 2, 4, 6, 8, 10 x 10^-4 M.
  2. Add 0.10 g charcoal to each; shake 45 min in the dark.
  3. Filter; measure absorbance of filtrate at 665 nm (or compare visually).
  4. From a calibration curve find equilibrium concentration c.
  5. Plot x/m vs c; read the plateau value a_max.
  6. Compute specific surface area using sigma = 130 A^2 per molecule.

Observations & Expected Results

Blue colour of filtrate fades with charcoal dose; the x/m vs c curve rises then plateaus at ~0.12 g dye per g charcoal, the classic Langmuir monolayer shape.

Worked Stoichiometric Calculations

Problem: 0.10 g charcoal adsorbs 12.0 mg methylene blue at the plateau (M = 319.9 g/mol, area per molecule 130 A^2). Estimate the specific surface area.

Working: Moles adsorbed = 0.0120/319.9 = 3.75 x 10^-5 mol. Molecules = 3.75 x 10^-5 x 6.022 x 10^23 = 2.26 x 10^19. Area = 2.26 x 10^19 x 130 x 10^-20 m^2 = 29.4 m^2 on 0.10 g, i.e. ~294 m^2/g - a typical value for activated charcoal.

Safety Precautions & Hazard Control

  • Keep dye solutions away from strong light (photobleaching).
  • Filter off all carbon fines before absorbance measurement.
  • Use the same charcoal particle size throughout.

Waste Disposal Protocol

Dye filtrates go to coloured organic waste; spent charcoal to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why does the curve plateau?

A: Once every surface site holds one dye molecule, no further monolayer adsorption is possible.

Q: Why is the molecular area of methylene blue assumed constant?

A: The flat aromatic molecule lies flat on graphitic surfaces, occupying a reproducible footprint.

Q: How does this compare with BET surface area?

A: It is a quick wet-chemistry estimate; BET with N2 gas is more precise but needs vacuum apparatus.

← Back to Experiments Directory