CHEMVEN

Lead-Acid Accumulator: Charging and Discharging

To cycle a small lead-acid cell and track voltage and acid density.

Level: UniversitySafety: Advanced lab onlyTime: 90 min
Aim of Experiment: To cycle a small lead-acid cell and track voltage and acid density.

Theoretical Foundations

Discharge: Pb + PbO2 + 2H2SO4 -> 2PbSO4 + 2H2O, Edeg = 1.69 - (-0.36) = 2.05 V. Charging reverses it. Because H2SO4 is consumed on discharge, the acid density falls - the basis of the hydrometer state-of-charge test.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Lead plates (one pasted with PbO2)
  • Beaker
  • DC supply with current limit
  • Voltmeter
  • Ammeter
  • Hydrometer or density measurement

Chemical Reagents

  • Sulphuric acid (2 M, battery acid strength for the model)
  • Distilled water (for topping up)
  • Sodium bicarbonate solution (for neutralising spills)

Step-by-Step Practical Procedure

  1. Assemble Pb|H2SO4|PbO2 and record the open-circuit voltage (~2.0 V).
  2. Discharge through a small bulb; record voltage vs time.
  3. Measure the acid density before and after discharge.
  4. Recharge at constant current, watching the voltage rise to ~2.4 V.
  5. Confirm the density recovers.

Observations & Expected Results

Discharge plateau ~2.0 V falling at the end; density drops measurably; recharge restores both.

Worked Stoichiometric Calculations

Problem: Calculate Edegcell from Edeg(PbO2/PbSO4) = +1.69 V and Edeg(PbSO4/Pb) = -0.36 V.

Working: Edegcell = 1.69 - (-0.36) = 2.05 V.

Safety Precautions & Hazard Control

  • H2SO4 is corrosive; wear gloves and eye protection.
  • Charging evolves H2 and O2 - ventilate, no sparks.
  • Switch off the power supply before changing any connections.

Waste Disposal Protocol

Lead plates and acid are hazardous waste; never pour down the drain.

Viva Voce Oral Defense Questions & Answers

Q: Why does the acid density indicate the state of charge?

A: Discharge consumes H2SO4 and produces water (see the cell reaction), so density falls in direct proportion to charge withdrawn.

Q: Why must a lead-acid battery never be left discharged?

A: PbSO4 recrystallises into large inactive crystals (sulphation), permanently reducing capacity.