CHEMVEN

Nickel Electroplating from a Watts Bath

To nickel-plate a steel object using a Watts-type bath and assess the deposit.

Level: UniversitySafety: Needs supervisionTime: 90 min
Aim of Experiment: To nickel-plate a steel object using a Watts-type bath and assess the deposit.

Theoretical Foundations

The Watts bath (NiSO4 + NiCl2 + H3BO3) deposits Ni2+ + 2e- -> Ni at the cathode. Boric acid buffers the pH; chloride improves anode dissolution. Nickel gives a hard, corrosion-resistant, decorative finish.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Steel strip (cathode)
  • Nickel anode
  • Beaker
  • DC supply
  • Ammeter
  • Balance
  • Thermometer

Chemical Reagents

  • Nickel sulphate
  • Nickel chloride
  • Boric acid
  • Distilled water

Step-by-Step Practical Procedure

  1. Make up the Watts bath (~250 g/L NiSO4, 45 g/L NiCl2, 30 g/L H3BO3) and warm to ~50 C.
  2. Clean and weigh the steel cathode.
  3. Plate at ~2 A for 30 minutes with mild agitation.
  4. Rinse, dry and re-weigh; inspect brightness and adhesion (tape test).
  5. Calculate the theoretical mass and current efficiency.

Observations & Expected Results

Bright silvery adherent nickel layer; typical gain ~1.05 g (theory 1.10 g), efficiency ~95%.

Worked Stoichiometric Calculations

Problem: Calculate the theoretical Ni mass for 2.0 A passed for 30 min (M = 58.7, n = 2).

Working: Q = 3600 C. m = 3600 x 58.7/(2 x 96485) = 211,320/192,970 = 1.095 g, about 1.10 g.

Safety Precautions & Hazard Control

  • Nickel salts are sensitisers; wear gloves.
  • Keep the bath near 50 C for best deposits.
  • Switch off the power supply before changing any connections.

Waste Disposal Protocol

Nickel baths are toxic to aquatic life; collect spent bath as heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: What is the role of boric acid?

A: It buffers the cathode film pH, preventing hydroxide precipitation that would give dull, brittle deposits.

Q: Why is chloride included in the Watts bath?

A: It promotes smooth dissolution of the nickel anode and raises bath conductivity.

← Back to Experiments Directory