CHEMVEN

Anodic Dissolution of Iron: Mass Loss by Faraday's Law

To verify Faraday's law for anodic dissolution by weighing iron lost from the anode.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To verify Faraday's law for anodic dissolution by weighing iron lost from the anode.

Theoretical Foundations

At the iron anode, Fe -> Fe2+ + 2e- (in non-oxidising media). The mass lost is m = Q x M/(nF) with M = 55.85 and n = 2. This is the basis of electrogravimetry and a model for corrosion mass loss.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Iron nail or plate anode
  • Copper or graphite cathode
  • Beaker
  • DC supply
  • Ammeter
  • Stopwatch
  • Balance

Chemical Reagents

  • Sodium sulphate solution (0.5 M, neutral electrolyte)
  • Distilled water (for rinsing)
  • Dilute HCl (for pre-cleaning the iron anode)

Step-by-Step Practical Procedure

  1. Weigh the iron anode accurately.
  2. Set up the cell in Na2SO4 solution.
  3. Pass 0.50 A for exactly 60 minutes.
  4. Remove, rinse, dry and re-weigh the anode.
  5. Compare the measured loss with Faraday's law.

Observations & Expected Results

Typical loss ~0.50-0.52 g versus theoretical 0.521 g.

Worked Stoichiometric Calculations

Problem: Calculate the theoretical iron loss for 0.50 A passed for 60 minutes (Fe -> Fe2+, M = 55.85).

Working: Q = 0.50 x 3600 = 1800 C. m = 1800 x 55.85/(2 x 96485) = 100,530/192,970 = 0.521 g.

Safety Precautions & Hazard Control

  • Loose corrosion products must be removed gently but fully before weighing.
  • Do not use chloride media (pitting complicates the mass balance).
  • Switch off the power supply before changing any connections.

Waste Disposal Protocol

The neutral Na2SO4 solution can go down the drain; iron sludge to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is Na2SO4 used rather than NaCl?

A: SO4(2-) is inert at the anode, while Cl- causes pitting and can evolve Cl2, complicating the mass balance.

Q: How does this relate to corrosion?

A: Corrosion is anodic dissolution driven by a galvanic cell instead of a power supply; the same m = Q M/(nF) relation converts corrosion current to mass loss.

← Back to Experiments Directory