Schweizer's Reagent (Cuprammonium Hydroxide)
To prepare Schweizer's reagent, [Cu(NH3)4](OH)2, which dissolves cellulose.
Theoretical Foundations
Freshly precipitated cupric hydroxide dissolves in concentrated ammonia: Cu(OH)2 + 4NH4OH → [Cu(NH3)4](OH)2 + 4H2O. The deep blue solution dissolves cellulose (cuprammonium rayon process) and is a classic test distinguishing silk from cotton.
Required Apparatus & Chemicals
Laboratory Apparatus
- 250 mL beaker
- Glass rod
- Funnel
- Filter paper
- Weighing balance
- Reagent bottle
- Test tubes
Chemical Reagents
- Copper sulfate pentahydrate, CuSO4·5H2O (24.97 g)
- Sodium hydroxide, NaOH (8.0 g)
- Concentrated ammonia solution (100 mL)
- Distilled water (150 mL)
- Cotton wool (for test)
Step-by-Step Practical Procedure
- Precipitate Cu(OH)2 cold from 24.97 g CuSO4·5H2O and 8.0 g NaOH as in the standard method.
- Filter and wash the blue precipitate free of sulfate.
- Transfer the moist precipitate to a beaker.
- Add 100 mL concentrated ammonia gradually with stirring; the precipitate dissolves to a deep blue solution.
- Filter into a reagent bottle and stopper.
- Test: a tuft of cotton wool dissolves in the reagent within minutes.
Observations & Expected Results
Deep blue viscous solution; dissolves cotton; copper content ~0.1 mol per batch.
Worked Stoichiometric Calculations
Problem: 9.76 g freshly precipitated Cu(OH)2 (M = 97.56) dissolves in excess ammonia. Calculate the theoretical mass of [Cu(NH3)4](OH)2 (M = 149.68) formed in solution.
Working: Moles Cu(OH)2 = 9.76/97.56 = 0.100 mol → 0.100 mol [Cu(NH3)4](OH)2. Theoretical mass = 0.100 × 149.68 = 15.0 g in solution.
Safety Precautions & Hazard Control
- Use freshly precipitated Cu(OH)2; aged hydroxide dissolves poorly.
- Concentrated ammonia fumes; ventilate well.
- Stopper the bottle; ammonia escapes on standing.
- Copper residues to heavy-metal waste.
Waste Disposal Protocol
Cuprammonium residues go to the heavy-metal inorganic waste container.
Viva Voce Oral Defense Questions & Answers
Q: Write the formation equation.
A: Cu(OH)2 + 4NH4OH → [Cu(NH3)4](OH)2 + 4H2O.
Q: Why does Schweizer's reagent dissolve cellulose?
A: The complex breaks cellulose hydrogen bonding, forming a soluble complex.
Q: Name the fibre made by this process.
A: Cuprammonium rayon.