CHEMVEN

Silica Gel by Acidification of Sodium Silicate

To prepare silica gel by precipitating silicic acid from water glass and drying it.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To prepare silica gel by precipitating silicic acid from water glass and drying it.

Theoretical Foundations

Hydrochloric acid decomposes sodium silicate: Na2SiO3 + 2HCl → H2SiO3↓ + 2NaCl. The gelatinous silicic acid, washed free of chloride and dried, gives porous silica gel: H2SiO3 →(Δ) SiO2 + H2O. Silica gel is a standard desiccant and chromatography adsorbent.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 500 mL beaker
  • Glass rod
  • Funnel
  • Filter paper
  • Weighing balance
  • Oven
  • Desiccator
  • Mortar and pestle

Chemical Reagents

  • Sodium silicate solution (water glass, 30 mL)
  • Concentrated hydrochloric acid (20 mL)
  • Distilled water (500 mL)
  • Cobalt chloride indicator (optional)

Step-by-Step Practical Procedure

  1. Dilute 30 mL water glass with 100 mL water.
  2. Add 20 mL concentrated HCl slowly with vigorous stirring.
  3. A gelatinous precipitate of silicic acid forms; continue stirring to break the gel.
  4. Allow to stand 15 minutes, then filter.
  5. Wash with hot water until free of chloride (test with AgNO3).
  6. Dry at 120 °C for 2 hours, then grind to granules.
  7. Store in an airtight container; test desiccant action on a damp salt.

Observations & Expected Results

White/translucent hard granules; strongly adsorb moisture.

Worked Stoichiometric Calculations

Problem: 12.2 g Na2SiO3 (M = 122.06) in the water glass reacts completely. Calculate the theoretical yield of SiO2 (M = 60.08). If 5.2 g of dry gel is obtained, find the percentage yield.

Working: Moles Na2SiO3 = 12.2/122.06 = 0.100 mol → 0.100 mol SiO2. Theoretical mass = 0.100 × 60.08 = 6.01 g. Percentage yield = (5.2/6.01) × 100 = 86.5%.

Safety Precautions & Hazard Control

  • Add acid with vigorous stirring to avoid lumps.
  • Wash thoroughly; residual NaCl reduces adsorptive capacity.
  • Dry fully at 120 °C to activate the gel.
  • Handle concentrated HCl with care.

Waste Disposal Protocol

Sodium chloride filtrate is flushed with water.

Viva Voce Oral Defense Questions & Answers

Q: Write the two reactions.

A: Na2SiO3 + 2HCl → H2SiO3 + 2NaCl; H2SiO3 → SiO2 + H2O.

Q: Why is silica gel a good desiccant?

A: Its huge porous surface area adsorbs water vapour physically.

Q: What does blue cobalt chloride silica gel indicate?

A: Blue = dry; pink = moist (hydrated cobalt chloride).

← Back to Experiments Directory