Cadmium Sulfide Yellow Pigment
To prepare cadmium sulfide, the brilliant yellow pigment, by precipitation.
Theoretical Foundations
Cadmium nitrate with hydrogen sulfide gives yellow CdS: Cd(NO3)2 + H2S → CdS↓ + 2HNO3. The precipitation is done in a fume cupboard. CdS ('cadmium yellow') is prized for its brilliance and permanence.
Required Apparatus & Chemicals
Laboratory Apparatus
- 250 mL beaker
- Gas delivery tube
- H2S generator (Kipp's)
- Funnel
- Filter paper
- Weighing balance
- Fume cupboard
Chemical Reagents
- Cadmium nitrate tetrahydrate, Cd(NO3)2·4H2O (30.85 g)
- Hydrogen sulfide gas
- Distilled water (150 mL)
Step-by-Step Practical Procedure
- Dissolve 30.85 g cadmium nitrate in 120 mL water in a fume cupboard.
- Pass H2S slowly through the solution with stirring.
- A bright yellow precipitate of CdS forms.
- Continue until precipitation is complete.
- Filter, wash with water until free of nitrate.
- Dry at 110 °C and weigh.
Observations & Expected Results
Brilliant yellow powder; typical yield 13.2–14.0 g.
Worked Stoichiometric Calculations
Problem: 30.85 g Cd(NO3)2·4H2O (M = 308.48) reacts with excess H2S. Calculate the theoretical yield of CdS (M = 144.46). If 13.6 g is obtained, find the percentage yield.
Working: Moles Cd(NO3)2·4H2O = 30.85/308.48 = 0.100 mol → 0.100 mol CdS. Theoretical mass = 0.100 × 144.46 = 14.45 g. Percentage yield = (13.6/14.45) × 100 = 94.1%.
Safety Precautions & Hazard Control
- Cadmium compounds are toxic and carcinogenic; wear gloves and a dust mask.
- H2S is toxic; fume cupboard mandatory.
- Avoid inhaling CdS dust.
- Collect all cadmium residues.
Waste Disposal Protocol
Cadmium residues go to the designated cadmium hazardous waste container.
Viva Voce Oral Defense Questions & Answers
Q: Write the precipitation equation.
A: Cd(NO3)2 + H2S → CdS + 2HNO3.
Q: Why is cadmium yellow prized by artists?
A: Brilliant colour, high opacity, and excellent permanence.
Q: What is the lattice structure of CdS?
A: Wurtzite (hexagonal) at room temperature.