CHEMVEN

Zinc Sulfide (Phosphor) by Precipitation

To prepare zinc sulfide phosphor by precipitation from zinc sulfate.

Level: UniversitySafety: Needs supervisionTime: 30 min
Aim of Experiment: To prepare zinc sulfide phosphor by precipitation from zinc sulfate.

Theoretical Foundations

Zinc sulfate with sodium sulfide gives white ZnS: ZnSO4 + Na2S → ZnS↓ + Na2SO4. Pure ZnS phosphoresces; doped with copper it glows green (used in luminous paints and X-ray screens). Precipitation must avoid acidic conditions that release H2S.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 250 mL beaker
  • Glass rod
  • Funnel
  • Filter paper
  • Weighing balance
  • Oven
  • Fume cupboard

Chemical Reagents

  • Zinc sulfate heptahydrate, ZnSO4·7H2O (28.75 g)
  • Sodium sulfide nonahydrate, Na2S·9H2O (24.02 g)
  • Distilled water (200 mL)

Step-by-Step Practical Procedure

  1. Dissolve 28.75 g ZnSO4·7H2O in 100 mL water.
  2. Dissolve 24.02 g Na2S·9H2O in 80 mL water in a fume cupboard.
  3. Add the sulfide solution to the zinc solution with stirring.
  4. A white precipitate of ZnS forms.
  5. Filter, wash thoroughly with water.
  6. Dry at 110 °C in the dark and weigh.
  7. Test phosphorescence: expose to light, then observe in the dark.

Observations & Expected Results

White powder; typical yield 8.9–9.4 g; faint afterglow in the dark.

Worked Stoichiometric Calculations

Problem: 28.75 g ZnSO4·7H2O (M = 287.54) reacts with excess Na2S. Calculate the theoretical yield of ZnS (M = 97.44). If 9.1 g is obtained, find the percentage yield.

Working: Moles ZnSO4·7H2O = 28.75/287.54 = 0.100 mol → 0.100 mol ZnS. Theoretical mass = 0.100 × 97.44 = 9.74 g. Percentage yield = (9.1/9.74) × 100 = 93.4%.

Safety Precautions & Hazard Control

  • Work in a fume cupboard; sulfide solutions release H2S if acidified.
  • Never add acid to the sulfide solution.
  • Wash the precipitate well.
  • Zinc residues to heavy-metal waste.

Waste Disposal Protocol

Sulfide-containing filtrates are oxidized with bleach before disposal.

Viva Voce Oral Defense Questions & Answers

Q: Why must the medium not be acidic?

A: Acid liberates toxic H2S: S(2−) + 2H+ → H2S.

Q: What makes ZnS phosphoresce?

A: Crystal defects and activator dopants (e.g., Cu) trap and slowly release excitation energy.

Q: Name the two crystal forms of ZnS.

A: Zinc blende (cubic) and wurtzite (hexagonal).

← Back to Experiments Directory