Zinc Chromate (Zinc Yellow) Pigment
To prepare zinc chromate pigment by precipitation.
Theoretical Foundations
Zinc sulfate with potassium chromate gives zinc chromate: ZnSO4 + K2CrO4 → ZnCrO4↓ + K2SO4. Zinc yellow was an important anticorrosive primer pigment for aircraft and steel.
Required Apparatus & Chemicals
Laboratory Apparatus
- 250 mL beaker
- Glass rod
- Funnel
- Filter paper
- Weighing balance
- Oven
Chemical Reagents
- Zinc sulfate heptahydrate, ZnSO4·7H2O (28.75 g)
- Potassium chromate, K2CrO4 (19.42 g)
- Distilled water (250 mL)
Step-by-Step Practical Procedure
- Dissolve 28.75 g ZnSO4·7H2O in 120 mL water.
- Dissolve 19.42 g K2CrO4 in 80 mL water.
- Add the chromate solution slowly with stirring.
- A yellow precipitate of ZnCrO4 forms.
- Filter, wash with hot water until free of sulfate.
- Dry at 110 °C, grind, and weigh.
Observations & Expected Results
Bright yellow powder; typical yield 16–17.5 g.
Worked Stoichiometric Calculations
Problem: 28.75 g ZnSO4·7H2O (M = 287.54) reacts with excess K2CrO4. Calculate the theoretical yield of ZnCrO4 (M = 181.38). If 16.8 g is obtained, find the percentage yield.
Working: Moles ZnSO4·7H2O = 28.75/287.54 = 0.100 mol → 0.100 mol ZnCrO4. Theoretical mass = 0.100 × 181.38 = 18.1 g. Percentage yield = (16.8/18.1) × 100 = 92.8%.
Safety Precautions & Hazard Control
- Chromate is carcinogenic; wear gloves and a dust mask.
- Avoid inhaling the pigment dust.
- Wash free of sulfate.
- Keep dry chromate away from organic matter.
Waste Disposal Protocol
Zinc/chromium residues go to the designated hazardous inorganic waste container.
Viva Voce Oral Defense Questions & Answers
Q: What was zinc chromate used for?
A: Anticorrosive primer for aircraft aluminium and steel.
Q: Why has its use declined?
A: Hexavalent chromium is carcinogenic.
Q: What is the oxidation state of Cr in ZnCrO4?
A: +6.