CHEMVEN

Magnesium Oxide by Burning Magnesium Ribbon

To prepare magnesium oxide by direct combustion of magnesium ribbon in air.

Level: UniversitySafety: Needs supervisionTime: 30 min
Aim of Experiment: To prepare magnesium oxide by direct combustion of magnesium ribbon in air.

Theoretical Foundations

Magnesium burns with a brilliant white flame: 2Mg + O2 →(Δ) 2MgO. A small amount of magnesium nitride also forms with atmospheric nitrogen: 3Mg + N2 → Mg3N4, which is removed by moistening and reheating (it hydrolyzes to MgO and NH3).

Required Apparatus & Chemicals

Laboratory Apparatus

  • Crucible with lid
  • Bunsen burner
  • Tongs
  • Weighing balance
  • Glass rod
  • Dropper

Chemical Reagents

  • Magnesium ribbon (2.43 g)
  • Distilled water (few drops)

Step-by-Step Practical Procedure

  1. Weigh a clean dry crucible with lid.
  2. Coil 2.43 g magnesium ribbon and place it in the crucible.
  3. Heat strongly with the lid slightly ajar until the ribbon ignites.
  4. Allow burning to complete; lift the lid briefly to admit air if needed.
  5. Moisten the product with a few drops of water and reheat to decompose any nitride.
  6. Cool in a desiccator, weigh, and calculate the mass of MgO formed.

Observations & Expected Results

Brilliant white flame; white powder residue; typical yield 3.8–4.0 g.

Worked Stoichiometric Calculations

Problem: 2.43 g Mg (M = 24.31) burns completely in air. Calculate the theoretical yield of MgO (M = 40.31). If 3.85 g is obtained, find the percentage yield.

Working: Moles Mg = 2.43/24.31 = 0.100 mol → 0.100 mol MgO. Theoretical mass = 0.100 × 40.31 = 4.03 g. Percentage yield = (3.85/4.03) × 100 = 95.5%.

Safety Precautions & Hazard Control

  • Never look directly at burning magnesium (intense UV light).
  • Keep the lid ajar, not sealed; pressure can build up.
  • Moisten and reheat to remove nitride impurity.
  • Handle the hot crucible with tongs.

Waste Disposal Protocol

Magnesium oxide is non-hazardous; dispose as solid inorganic waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is the product moistened and reheated?

A: To hydrolyze Mg3N4 impurity: Mg3N4 + 6H2O → 3Mg(OH)2 + 2NH3, then Mg(OH)2 → MgO + H2O.

Q: Why must you not look directly at the flame?

A: It emits intense ultraviolet light that damages the eyes.

Q: What is magnesia used for?

A: Refractory linings, antacids, and Sorel cement.

← Back to Experiments Directory