CHEMVEN

Water Glass: Fusion of Silica with Sodium Carbonate

To prepare sodium silicate (water glass) by fusing sand with sodium carbonate.

Level: UniversitySafety: Needs supervisionTime: 90 min
Aim of Experiment: To prepare sodium silicate (water glass) by fusing sand with sodium carbonate.

Theoretical Foundations

Silica is an acidic oxide that displaces CO2 from sodium carbonate at high temperature: Na2CO3 + SiO2 →(fusion) Na2SiO3 + CO2↑. The glassy melt dissolves in water under pressure (or prolonged boiling) to give water glass solution, used as an adhesive and preservative.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Fireclay crucible
  • Furnace or blast burner
  • Tongs
  • Iron plate
  • Beaker
  • Glass rod
  • Weighing balance

Chemical Reagents

  • Anhydrous sodium carbonate, Na2CO3 (10.6 g)
  • Fine clean sand, SiO2 (6.0 g)
  • Distilled water (100 mL)

Step-by-Step Practical Procedure

  1. Mix 10.6 g sodium carbonate intimately with 6.0 g fine sand.
  2. Transfer to a fireclay crucible and heat strongly in a furnace until a clear melt forms.
  3. Pour the melt onto a clean iron plate and allow to solidify.
  4. Break the glassy solid into small pieces and weigh.
  5. Boil the pieces with 100 mL water for 30 minutes to obtain water glass solution.
  6. Filter and store the viscous solution in a stoppered bottle.

Observations & Expected Results

Transparent glassy lumps; dissolve to a viscous, strongly alkaline solution.

Worked Stoichiometric Calculations

Problem: 10.6 g Na2CO3 (M = 105.99) is fused with excess sand. Calculate the theoretical yield of sodium metasilicate Na2SiO3 (M = 122.06).

Working: Moles Na2CO3 = 10.6/105.99 = 0.100 mol → 0.100 mol Na2SiO3. Theoretical mass = 0.100 × 122.06 = 12.2 g.

Safety Precautions & Hazard Control

  • Wear heat-resistant gloves and a face shield during fusion.
  • Heat gradually at first; the charge may froth as CO2 escapes.
  • Do not touch the hot crucible with bare hands.
  • Add water to the glassy solid cautiously; it dissolves exothermically.

Waste Disposal Protocol

Silicate solution is strongly alkaline; neutralize before disposal.

Viva Voce Oral Defense Questions & Answers

Q: Why is sodium silicate called water glass?

A: The fused solid looks like glass but dissolves in water.

Q: Write the fusion reaction.

A: Na2CO3 + SiO2 → Na2SiO3 + CO2.

Q: Name two uses of water glass.

A: As an adhesive for paper/board and as a preservative coating for eggs and concrete.

← Back to Experiments Directory