Plaster of Paris from Gypsum (Controlled Calcination)

To prepare plaster of Paris by controlled heating of gypsum and verify its setting property.

Level: UniversitySafety: SafeTime: 90 min
Aim of Experiment: To prepare plaster of Paris by controlled heating of gypsum and verify its setting property.

Theoretical Foundations

Gypsum (CaSO4·2H2O) heated to 120–130 °C loses three-quarters of its water of crystallization: 2CaSO4·2H2O →(393 K) 2CaSO4·½H2O + 3H2O. Overheating above 200 °C gives dead-burnt anhydrite that does not set. Mixed with water, plaster rehydrates and sets to hard gypsum.

Required Apparatus & Chemicals

Laboratory Apparatus

  • China dish
  • Oven or sand bath
  • Thermometer (0–200 °C)
  • Weighing balance
  • Glass rod
  • Desiccator
  • Mortar and pestle

Chemical Reagents

  • Powdered gypsum, CaSO4·2H2O (34.4 g)
  • Distilled water (for setting test)

Step-by-Step Practical Procedure

  1. Weigh 34.4 g powdered gypsum into a china dish.
  2. Heat in an oven or on a sand bath, maintaining 120–130 °C for 1 hour with occasional stirring.
  3. Cool in a desiccator and weigh; the mass loss corresponds to 1.5 molecules of water.
  4. Grind to a fine powder if lumpy.
  5. Setting test: mix a little product with water to a paste and note that it sets hard within minutes.
  6. Store the product in an airtight container.

Observations & Expected Results

White powder; mass loss ~7.2 g; paste sets to a hard mass in 5–10 minutes.

Worked Stoichiometric Calculations

Problem: 34.4 g gypsum CaSO4·2H2O (M = 172.17) is heated at 125 °C. Calculate the theoretical mass of plaster of Paris CaSO4·½H2O (M = 145.15) and the expected mass loss.

Working: Moles gypsum = 34.4/172.17 = 0.200 mol → 0.200 mol plaster. Theoretical mass = 0.200 × 145.15 = 29.0 g. Mass loss = 34.4 − 29.0 = 5.4 g (water lost = 0.300 mol × 18.0 = 5.4 g).

Safety Precautions & Hazard Control

  • Control the temperature strictly between 120 and 130 °C.
  • Stir occasionally for uniform heating.
  • Cool in a desiccator to prevent rehydration.
  • Store airtight; plaster absorbs moisture from air.

Waste Disposal Protocol

No hazardous waste; excess gypsum/plaster can go to general solid waste.

Viva Voce Oral Defense Questions & Answers

Q: What is the chemical formula of plaster of Paris?

A: CaSO4·½H2O (calcium sulfate hemihydrate).

Q: What happens if gypsum is heated above 200 °C?

A: It forms dead-burnt anhydrous CaSO4, which does not set with water.

Q: Why does plaster of Paris set with water?

A: It rehydrates to interlocking gypsum crystals: CaSO4·½H2O + 1½H2O → CaSO4·2H2O.