CHEMVEN

Blowpipe Reduction on Charcoal: Extracting Metals from Salts

Extract metallic copper, tin and lead beads from their salts by charcoal reduction.

Level: UniversitySafety: Needs supervisionTime: 40 min
Aim of Experiment: Extract metallic copper, tin and lead beads from their salts by charcoal reduction.

Theoretical Foundations

C + metal oxide → metal + CO/CO₂ at blowpipe temperatures. With Na₂CO₃ flux: CuO → red copper bead; SnO₂ → white tin bead (hard, 'tin cry' when bent); PbO → soft grey lead bead. The bead's colour, hardness and malleability identify the metal — the prospector's classical assay in miniature.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Blowpipe
  • Bunsen burner
  • Charcoal block
  • Sodium carbonate

Chemical Reagents

  • CuO or CuSO₄
  • SnO₂ or SnCl₂
  • PbO or Pb(NO₃)₂
  • Anhydrous Na₂CO₃

Step-by-Step Practical Procedure

  1. Mix each oxide/salt with Na₂CO₃ in separate charcoal cavities.
  2. Reduce with the blowpipe's reducing flame for 2–3 min each.
  3. Recover the beads; test hardness and malleability.
  4. Tin: bend the bead and listen for the 'tin cry'.
  5. Record bead properties in a table.

Observations & Expected Results

Cu red malleable bead; Sn white bead with tin cry; Pb soft grey bead marking paper.

Worked Stoichiometric Calculations

Problem: 2CuO + C → 2Cu + CO₂. What mass of Cu from 1.00 g CuO? (illustrative)

Working: 1.00 g CuO = 0.0126 mol → 0.0126 mol Cu = 0.80 g.

Safety Precautions & Hazard Control

  • Intense heat — eye protection, tongs.
  • Lead fumes — ventilate, tiny amounts.
  • Wear safety goggles and a lab coat throughout the experiment.

Waste Disposal Protocol

Metal beads and charcoal to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: What causes the 'tin cry'?

A: Twinning of tin crystals deforming — an audible creak unique to tin.

Q: Why add Na₂CO₃?

A: Flux: lowers melting behaviour and converts salts to reducible carbonates/oxides.

← Back to Experiments Directory