CHEMVEN

Eutectic Arrest: Cooling Curve of Tin-Lead Solder

To record the cooling curve of 60/40 solder and identify the eutectic halt at 183 °C.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To record the cooling curve of 60/40 solder and identify the eutectic halt at 183 °C.

Theoretical Foundations

Off-eutectic alloys freeze over a range: primary crystals separate first (sloped cooling), then the remaining liquid solidifies at the eutectic temperature with a flat thermal arrest. Near-eutectic 60/40 Sn-Pb shows only a tiny primary arrest before the long 183 °C eutectic plateau where liquid → α(Pb-rich) + β(Sn-rich) — the basis of thermal analysis for phase diagrams.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Crucible
  • Thermocouple (to 350 °C)
  • Bunsen burner
  • Stopwatch
  • Tongs
  • Heat-resistant mat

Chemical Reagents

  • 60/40 Sn-Pb solder (about 30 g)
  • Lead-containing: handle with gloves
  • Borax flux (a pinch, to keep the melt clean)

Step-by-Step Practical Procedure

  1. Melt the solder in the crucible and insert the thermocouple.
  2. Remove from heat and record temperature every 15 seconds.
  3. Plot temperature versus time.
  4. Identify the short primary arrest and the long eutectic plateau.
  5. Read the plateau temperature and compare with 183 °C.
  6. Discuss how the curve would differ for pure tin (single sharp arrest).

Observations & Expected Results

Cooling slows near 190 °C (primary Sn-rich crystals), then the temperature locks at about 183 °C for minutes during eutectic solidification before falling again.

Worked Stoichiometric Calculations

Problem: The eutectic plateau lasts 6.0 min with heat loss 40 J min⁻¹ for 30 g of solder. Estimate the latent heat per gram.

Working: Heat = 6.0 × 40 = 240 J. Per gram: 240/30 = 8.0 J g⁻¹ released during eutectic freezing.

Safety Precautions & Hazard Control

  • Lead fumes: ventilate; wear gloves.
  • Molten solder burns; tongs only.
  • Do not overheat above 350 °C.
  • Wash hands after handling lead.

Waste Disposal Protocol

Solidified solder is collected as lead-containing metal waste.

Viva Voce Oral Defense Questions & Answers

Q: What is a eutectic arrest?

A: The flat temperature halt during simultaneous crystallization of two solids from the eutectic liquid.

Q: Why is there a short arrest before the plateau?

A: Primary (Sn-rich) crystals freeze over a temperature range before the remaining liquid reaches eutectic composition.

Q: How would pure tin's curve differ?

A: A single sharp plateau at 232 °C with no preceding slope.

← Back to Experiments Directory