CHEMVEN

Lead-Acid Cell: A Rechargeable 2 V System

To build a small lead-acid cell, measure its ~2.0 V EMF, and demonstrate rechargeability.

Level: UniversitySafety: Advanced lab onlyTime: 75 min
Aim of Experiment: To build a small lead-acid cell, measure its ~2.0 V EMF, and demonstrate rechargeability.

Theoretical Foundations

Discharge: Pb + PbO2 + 2H2SO4 → 2PbSO4 + 2H2O (E° ≈ 2.04 V per cell; six cells give a 12 V battery). Charging reverses it. Both electrodes become PbSO4 on discharge — the acid is consumed, so specific gravity tracks charge state. Lead and sulfuric acid demand advanced-lab handling.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Small beaker
  • Lead strips (2)
  • DC supply for charging
  • Voltmeter
  • Hydrometer (optional)
  • Gloves, goggles, apron

Chemical Reagents

  • Sulfuric acid, about 2 M (about 100 mL)
  • Lead strips (2, about 10 g each)
  • Sodium bicarbonate (for neutralizing spills)

Step-by-Step Practical Procedure

  1. Wearing full PPE, place two lead strips in 2 M H2SO4 (do not let them touch).
  2. Measure the initial voltage (low, unformed plates).
  3. Charge at low current (0.2 A) for 20 minutes: one plate darkens (PbO2).
  4. Measure the EMF — now about 2.0 V.
  5. Discharge through a small bulb and watch the voltage fall.
  6. Recharge and confirm the voltage recovers.

Observations & Expected Results

After forming, the cell gives ~2.0 V, lights the bulb, and recovers on recharge — a true secondary cell in miniature.

Worked Stoichiometric Calculations

Problem: A 12 V car battery contains 6 cells. What is the voltage per cell, and how many moles of H2SO4 are consumed per mole of Pb discharged?

Working: 12/6 = 2.0 V per cell. From the equation: 2 mol H2SO4 per mol Pb.

Safety Precautions & Hazard Control

  • Sulfuric acid is severely corrosive; full PPE and a fume hood.
  • Lead is toxic; wear gloves, wash hands.
  • Charging releases hydrogen — no flames, ventilate.
  • Neutralize spills with sodium bicarbonate.

Waste Disposal Protocol

Acid must be neutralized and lead collected as hazardous waste — never down the drain.

Viva Voce Oral Defense Questions & Answers

Q: Write the overall cell reaction.

A: Pb + PbO2 + 2H2SO4 ⇌ 2PbSO4 + 2H2O (discharge →, charge ←).

Q: How can you tell the state of charge?

A: Acid specific gravity falls on discharge as H2SO4 is consumed.

Q: Why must both plates be lead compounds?

A: Both electrodes convert to PbSO4 on discharge; charging regenerates Pb and PbO2.

← Back to Experiments Directory