CHEMVEN

Verdigris Patina: Growing Basic Copper Carbonate on Copper

To grow an artificial verdigris patina on copper and identify it as basic copper carbonate/acetate.

Level: UniversitySafety: Needs supervisionTime: 20 min setup + 7 days
Aim of Experiment: To grow an artificial verdigris patina on copper and identify it as basic copper carbonate/acetate.

Theoretical Foundations

Copper exposed to air, moisture, and CO2 slowly forms a green patina of basic copper carbonates (e.g., malachite Cu2(OH)2CO3) — the color of the Statue of Liberty. Vinegar vapor (acetic acid) accelerates the process by first forming copper acetate, which converts to carbonate. The patina is adherent and protective (passivating).

Required Apparatus & Chemicals

Laboratory Apparatus

  • 2 copper strips or coins
  • 2 jars with lids
  • Paper towel
  • Emery paper

Chemical Reagents

  • Vinegar (acetic acid, a few mL)
  • Table salt (a pinch, optional accelerator)
  • Copper strips (2)

Step-by-Step Practical Procedure

  1. Clean both copper strips bright with emery paper.
  2. Crumple damp paper towel in jar 1, add a few mL of vinegar, and suspend strip 1 above the liquid (not touching).
  3. Place strip 2 in jar 2 with damp towel but no vinegar (control).
  4. Seal both and leave 7 days.
  5. Compare colors: verdigris green versus slow brown tarnish.
  6. Scrape a little patina and test its effervescence with a drop of acid (carbonate test).

Observations & Expected Results

The vinegar-exposed strip develops a blue-green crust within days; the control only dulls brown; the crust fizzes with acid, confirming carbonate.

Worked Stoichiometric Calculations

Problem: Malachite is Cu2(OH)2CO3 (M = 221.12). What mass of CO2 is fixed per 10.0 g of malachite patina?

Working: Moles = 10.0/221.12 = 0.04522 mol. CO2 = 0.04522 × 44.01 = 1.99 g.

Safety Precautions & Hazard Control

  • Vinegar vapors are mild; ventilate.
  • Copper salts are toxic; wear gloves when scraping patina.
  • Wash hands after handling.

Waste Disposal Protocol

Patina scrapings go in solid chemical waste; vinegar goes down the drain.

Viva Voce Oral Defense Questions & Answers

Q: What is the green patina on old copper roofs?

A: Basic copper carbonates/sulfates, mainly brochantite and malachite-type phases.

Q: Why is the patina protective?

A: It is adherent and insoluble, sealing the metal from further attack (passivation).

Q: What role does vinegar play?

A: Acetic acid accelerates initial copper dissolution; the acetate converts to carbonate in air.

← Back to Experiments Directory