CHEMVEN

Titanium White: Covering Power of TiO2 Pigment

To compare the hiding (covering) power of titanium white with zinc white and chalk, relating it to refractive index.

Level: UniversitySafety: SafeTime: 40 min
Aim of Experiment: To compare the hiding (covering) power of titanium white with zinc white and chalk, relating it to refractive index.

Theoretical Foundations

Hiding power comes from light scattering at pigment-binder interfaces, which scales with the refractive-index contrast. Rutile TiO2 has n ≈ 2.7, far above typical binders (n ≈ 1.5), so it hides superbly; ZnO (n ≈ 2.0) is weaker and chalk CaCO3 (n ≈ 1.6) barely hides at all. This is why TiO2 dominates white paints.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 3 glass slides
  • Paintbrushes
  • Black-and-white hiding-power chart (printed)
  • Balance

Chemical Reagents

  • Titanium dioxide powder (a few grams)
  • Zinc oxide powder (a few grams)
  • Chalk/calcium carbonate powder (a few grams)
  • Clear binder (PVA glue diluted, or linseed oil)

Step-by-Step Practical Procedure

  1. Make three paints with equal pigment loading in the binder.
  2. Brush one stripe of each across the black-white chart boundary.
  3. Let dry and compare how well the black is hidden.
  4. Rank the hiding power.
  5. Look up the refractive indices and correlate.
  6. Discuss why nano-TiO2 (sunscreen grade) hides poorly.

Observations & Expected Results

TiO2 white obliterates the black/white boundary; ZnO partly hides; chalk is nearly transparent over black — ranking follows refractive index.

Worked Stoichiometric Calculations

Problem: Scattering scales roughly with (n(pigment) − n(binder))². Compare TiO2 (2.7) and chalk (1.6) in binder n = 1.5.

Working: TiO2: (2.7 − 1.5)² = 1.44. Chalk: (1.6 − 1.5)² = 0.01 — a 144× contrast in scattering strength.

Safety Precautions & Hazard Control

  • Powders: avoid inhaling dust; wear a dust mask if sensitive.
  • No significant chemical hazards.
  • Wash brushes before paint dries.

Waste Disposal Protocol

Dried paint solids are general waste; wash water goes down the drain.

Viva Voce Oral Defense Questions & Answers

Q: Why does TiO2 hide so well?

A: Its very high refractive index (≈ 2.7) gives huge scattering at each pigment-binder interface.

Q: Why is chalk a poor white pigment?

A: Its refractive index (≈ 1.6) nearly matches binders, so little scattering occurs.

Q: Why is sunscreen TiO2 transparent?

A: Nanoparticles much smaller than light's wavelength scatter visible light weakly (Rayleigh regime).

← Back to Experiments Directory