Silica Gel from Water Glass: Precipitation and Drying Power

To precipitate silica gel from sodium silicate with acid, wash it, and test its desiccant power against a control.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To precipitate silica gel from sodium silicate with acid, wash it, and test its desiccant power against a control.

Theoretical Foundations

Acidifying sodium silicate gives silicic acid, which polymerizes: Na2SiO3 + 2HCl → SiO2·nH2O + 2NaCl + H2O. The washed, dried product is porous silica gel with hundreds of m² g⁻¹ surface area; its pores adsorb water vapor, making it the familiar packet desiccant that can be regenerated by heating.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 250 mL beaker
  • Stirrer
  • pH paper
  • Filter funnel
  • Oven (110 °C)
  • 2 sealed jars
  • Balance

Chemical Reagents

  • Sodium silicate solution (about 50 mL)
  • Hydrochloric acid, about 2 M (about 40 mL)
  • Distilled water
  • Cobalt chloride paper or a damp sponge (humidity test)

Step-by-Step Practical Procedure

  1. Dilute 50 mL water glass with 50 mL water.
  2. Add 2 M HCl slowly with stirring until pH ≈ 7; a white gel precipitates.
  3. Filter and wash the gel free of chloride (test washings with AgNO3).
  4. Dry at 110 °C for 2 hours.
  5. Weigh dry gel into a dish in a sealed jar with a damp sponge; weigh a control dish without gel.
  6. After 24 h, reweigh both to compare water uptake.

Observations & Expected Results

A voluminous white gel forms, dries to gritty translucent granules, and gains several percent mass in the humid jar while the control barely changes.

Worked Stoichiometric Calculations

Problem: 5.0 g of dry gel gains 1.1 g in 24 h. What is its water uptake in percent and in mmol g⁻¹?

Working: Uptake = 1.1/5.0 × 100% = 22%. Moles water per gram = (1.1/18.015)/5.0 = 0.0122 mol g⁻¹ = 12.2 mmol g⁻¹.

Safety Precautions & Hazard Control

  • HCl is corrosive; wear goggles and gloves.
  • Hot oven: use tongs.
  • Wash the gel well; residual acid or salt ruins desiccant performance.

Waste Disposal Protocol

Neutralize acidic filtrates before drain disposal; silica gel is general waste.

Viva Voce Oral Defense Questions & Answers

Q: Why must chloride be washed out?

A: Residual NaCl fills pores and the gel stays damp, destroying desiccant capacity.

Q: How is silica gel regenerated?

A: Heating to about 110-150 °C drives off adsorbed water.

Q: Why does the gel adsorb water?

A: Its huge internal pore surface binds water molecules by hydrogen bonding and capillary condensation.