CHEMVEN

Cement Setting: Water-Cement Ratio Controls Strength

To show that a lower water-cement ratio gives stronger hardened cement paste, and to follow the exothermic hydration.

Level: UniversitySafety: Needs supervisionTime: 30 min setup + 7 days curing
Aim of Experiment: To show that a lower water-cement ratio gives stronger hardened cement paste, and to follow the exothermic hydration.

Theoretical Foundations

Portland cement's calcium silicates hydrate: 2Ca3SiO5 + 6H2O → Ca3Si2O7·3H2O (C-S-H gel) + 3Ca(OH)2. The C-S-H gel binds everything; excess water leaves pores that weaken the product, so strength falls as the water-cement (w/c) ratio rises. Typical structural concrete uses w/c ≈ 0.4-0.5.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 3 paper cups (molds)
  • Balance
  • Measuring cylinder
  • Thermometer
  • Stirring sticks
  • Bathroom scale or weights for strength test

Chemical Reagents

  • Portland cement (about 600 g)
  • Water
  • Mold-release oil (thin smear, for easy demolding)

Step-by-Step Practical Procedure

  1. Mix three pastes with w/c = 0.35, 0.50, 0.65 (e.g., 200 g cement with 70, 100, 130 mL water).
  2. Record the temperature rise during the first hour (exothermic hydration).
  3. Cast each paste into a labeled cup and level the surface.
  4. Cure 7 days in a damp covered tray.
  5. Demold and compare hardness by scratching and by loading with weights until cracking.
  6. Rank strengths against w/c ratio.

Observations & Expected Results

The 0.35 paste sets hardest with least bleeding; the 0.65 paste is visibly porous and crumbles under load — strength falls steeply with w/c.

Worked Stoichiometric Calculations

Problem: How much water is needed for 200 g of cement at w/c = 0.45?

Working: Water = 0.45 × 200 g = 90 g ≈ 90 mL.

Safety Precautions & Hazard Control

  • Wet cement is caustic (pH ~13); wear gloves and goggles.
  • Do not wash cement down the drain in quantity — it sets in pipes.
  • Avoid inhaling cement dust.

Waste Disposal Protocol

Let washings settle, decant water, and bin the solid residue as construction waste.

Viva Voce Oral Defense Questions & Answers

Q: What is C-S-H gel?

A: Calcium silicate hydrate gel — the main binding product of cement hydration.

Q: Why does extra water weaken concrete?

A: Unreacted water leaves capillary pores, reducing load-bearing cross-section.

Q: Is cement setting just drying?

A: No — it is chemical hydration forming new compounds; it hardens even underwater.

← Back to Experiments Directory