Zinc Oxide Nanoparticles by Precipitation: UV Absorption Edge
To precipitate ZnO nanoparticles and locate their UV absorption edge near the 3.3 eV band gap.
Theoretical Foundations
Adding NaOH to zinc acetate precipitates Zn(OH)2, which dehydrates on warming to ZnO nanoparticles (Zn(CH3COO)2 + 2NaOH → ZnO + 2CH3COONa + H2O). ZnO's direct band gap of 3.3 eV gives a sharp absorption edge near 375 nm; nanoparticle samples show the edge slightly blue-shifted by quantum confinement, measurable with a UV spectrometer.
Required Apparatus & Chemicals
Laboratory Apparatus
- 250 mL beaker
- Hot plate with stirrer
- UV-vis spectrometer
- Cuvettes
- pH paper
- Filter paper
Chemical Reagents
- Zinc acetate dihydrate (about 2.2 g)
- Sodium hydroxide (about 0.8 g)
- Ethanol or distilled water (about 150 mL)
Step-by-Step Practical Procedure
- Dissolve 2.2 g zinc acetate dihydrate in 100 mL warm ethanol/water.
- Dissolve 0.8 g NaOH in 50 mL of the same solvent.
- Add the NaOH solution dropwise with vigorous stirring; a white precipitate of Zn(OH)2 forms.
- Heat to 70 °C for 30 minutes to convert it to ZnO.
- Record the UV-vis spectrum of a diluted suspension.
- Locate the absorption edge (steep rise near 360-380 nm) and convert to eV.
Observations & Expected Results
The white suspension's spectrum climbs steeply below about 375 nm; the edge corresponds to about 3.3 eV, the ZnO band gap.
Worked Stoichiometric Calculations
Problem: The absorption edge is at 375 nm. Calculate the band gap in eV.
Working: E = 1240/375 = 3.31 eV — the textbook ZnO band gap.
Safety Precautions & Hazard Control
- NaOH is caustic; wear goggles and gloves.
- Hot ethanol is flammable; use a water bath, no open flame.
- Avoid inhaling fine ZnO powder.
Waste Disposal Protocol
Collect ZnO suspensions as inorganic waste; do not pour large amounts down the drain.
Viva Voce Oral Defense Questions & Answers
Q: Why does ZnO absorb at 375 nm?
A: Photons with energy ≥ the 3.3 eV band gap excite electrons from valence to conduction band.
Q: What is the chemical sequence in this synthesis?
A: Precipitation of Zn(OH)2 followed by thermal dehydration to ZnO.
Q: Why might nanoparticles show a slightly larger gap than bulk?
A: Quantum confinement widens the gap in very small particles.