Ferrofluid: Magnetic Nanoparticles That Spike

To synthesize magnetite (Fe3O4) nanoparticles by coprecipitation, stabilize a ferrofluid, and observe Rosensweig spikes in a magnetic field.

Level: UniversitySafety: Needs supervisionTime: 75 min
Aim of Experiment: To synthesize magnetite (Fe3O4) nanoparticles by coprecipitation, stabilize a ferrofluid, and observe Rosensweig spikes in a magnetic field.

Theoretical Foundations

Coprecipitating Fe²⁺ and Fe³⁺ in a 1:2 ratio with ammonia gives Fe3O4 nanoparticles (Fe²⁺ + 2Fe³⁺ + 8OH⁻ → Fe3O4 + 4H2O). Below about 20 nm the particles are superparamagnetic single domains; coated with surfactant (oleic acid) in oil they form a ferrofluid that spikes along field lines when a magnet approaches — the normal-field instability.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 250 mL beaker
  • Stirrer/hot plate
  • Strong neodymium magnet
  • Petri dish
  • Filter funnel
  • pH paper

Chemical Reagents

  • Iron(II) sulfate heptahydrate FeSO4·7H2O (about 2.8 g)
  • Iron(III) chloride hexahydrate FeCl3·6H2O (about 5.4 g)
  • Ammonia solution, concentrated (about 20 mL)
  • Oleic acid (about 2 mL)
  • Kerosene or light oil (about 30 mL)
  • Distilled water

Step-by-Step Practical Procedure

  1. Dissolve 2.8 g FeSO4·7H2O and 5.4 g FeCl3·6H2O in 100 mL distilled water.
  2. With vigorous stirring, add concentrated ammonia until pH 10-11; black Fe3O4 precipitates.
  3. Warm to 70 °C for 20 minutes with stirring.
  4. Add 2 mL oleic acid and stir 15 minutes to coat the particles.
  5. Let the black solid settle, decant, and wash twice with water.
  6. Disperse the coated particles in 30 mL kerosene with shaking.
  7. Pour a shallow pool in a petri dish and bring the magnet underneath to see spikes.

Observations & Expected Results

A black oily fluid forms; near the magnet it erupts into sharp spikes aligned with the field, collapsing when the magnet is removed.

Worked Stoichiometric Calculations

Problem: Check the Fe²⁺:Fe³⁺ mole ratio used: 2.8 g FeSO4·7H2O (M = 278.01) and 5.4 g FeCl3·6H2O (M = 270.30).

Working: Fe²⁺: 2.8/278.01 = 0.01007 mol. Fe³⁺: 5.4/270.30 = 0.01998 mol. Ratio ≈ 1:1.98 ≈ 1:2, as required for Fe3O4.

Safety Precautions & Hazard Control

  • Concentrated ammonia is corrosive to eyes and lungs; use a fume hood.
  • Neodymium magnets pinch hard and damage electronics.
  • Kerosene is flammable; keep away from flames.
  • Wear gloves throughout.

Waste Disposal Protocol

Collect the oil-based ferrofluid and washings as chemical waste; do not pour oil down the drain.

Viva Voce Oral Defense Questions & Answers

Q: Why must the Fe²⁺:Fe³⁺ ratio be 1:2?

A: Magnetite is FeO·Fe2O3, containing one Fe²⁺ per two Fe³⁺.

Q: What is superparamagnetism?

A: Single-domain nanoparticles whose magnetization flips thermally, so they magnetize only in an applied field with no remanence.

Q: What does the oleic acid do?

A: It coats the particles (surfactant), preventing agglomeration and letting them disperse in oil.