CHEMVEN

Electroplating Copper onto Iron: A Protective Metallic Coating

To electroplate a uniform copper layer onto an iron nail and use Faraday's law to predict the mass deposited.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To electroplate a uniform copper layer onto an iron nail and use Faraday's law to predict the mass deposited.

Theoretical Foundations

In a CuSO4/H2SO4 bath with a copper anode, Cu²⁺ + 2e⁻ → Cu deposits on the iron cathode. The mass follows Faraday's law: m = Q·M/(n·F) = I·t·M/(n·F). A coherent copper coat protects iron by barrier action (as long as it is pore-free, since copper is cathodic to iron).

Required Apparatus & Chemicals

Laboratory Apparatus

  • DC power supply (0-6 V)
  • Beaker (250 mL)
  • Copper strip (anode)
  • Iron nail (cathode)
  • Connecting wires
  • Balance (0.001 g)
  • Ammeter

Chemical Reagents

  • Copper(II) sulfate pentahydrate (about 25 g)
  • Dilute sulfuric acid, about 1 M (a few mL)
  • Distilled water (about 200 mL)
  • Iron nail
  • Copper strip

Step-by-Step Practical Procedure

  1. Clean the nail with emery paper, weigh it accurately.
  2. Make the bath: 25 g CuSO4·5H2O in 200 mL water plus a few mL of dilute H2SO4.
  3. Connect the nail as cathode (−) and copper strip as anode (+).
  4. Apply about 0.5 A for 30 minutes, keeping electrodes apart.
  5. Remove, rinse, dry, and reweigh the nail.
  6. Compare the measured gain with Faraday's law prediction.
  7. Inspect the coating for uniformity and adhesion (tape test).

Observations & Expected Results

The nail gains a smooth pink copper coat; the mass gain closely matches the Faraday prediction when current efficiency is high.

Worked Stoichiometric Calculations

Problem: At 0.50 A for 30 min, what mass of copper should deposit? (Cu = 63.55, F = 96485)

Working: Q = 0.50 × 1800 = 900 C. Moles Cu = 900/(2 × 96485) = 0.004664 mol. Mass = 0.004664 × 63.55 = 0.296 g.

Safety Precautions & Hazard Control

  • Dilute sulfuric acid is corrosive; wear goggles and gloves.
  • Do not short-circuit the power supply.
  • Keep electrical connections dry.
  • Copper sulfate solution is toxic to aquatic life — collect waste.

Waste Disposal Protocol

The plating bath is collected for heavy-metal waste; rinse water is diluted heavily or collected per local rules.

Viva Voce Oral Defense Questions & Answers

Q: State Faraday's first law of electrolysis.

A: Mass deposited is proportional to the quantity of electricity passed: m = Q·M/(n·F).

Q: Why is the copper anode used instead of an inert one?

A: It dissolves to replenish Cu²⁺, keeping the bath concentration constant.

Q: Why must the coat be pore-free?

A: Copper is cathodic to iron, so any pore exposes iron as a small anode and accelerates local rusting.

← Back to Experiments Directory