CHEMVEN

Sacrificial Anodes: Zinc Protecting Iron in Salt Water

To demonstrate cathodic protection by coupling iron to a zinc sacrificial anode in salt water.

Level: UniversitySafety: Needs supervisionTime: 25 min setup + 7 days observation
Aim of Experiment: To demonstrate cathodic protection by coupling iron to a zinc sacrificial anode in salt water.

Theoretical Foundations

When zinc and iron are in electrical contact in an electrolyte, they form a galvanic cell. Zinc (E° = −0.76 V) is the anode and dissolves (Zn → Zn²⁺ + 2e⁻), supplying electrons that keep iron (E° = −0.44 V) cathodic so it cannot oxidize. The zinc is 'sacrificed' and must be replaced periodically — the principle protecting ship hulls and pipelines.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 2 beakers
  • 2 iron nails
  • Zinc strip
  • Copper wire
  • Salt water (3.5% NaCl)

Chemical Reagents

  • Sodium chloride solution, 3.5% (about 400 mL)
  • Iron nails (2)
  • Zinc strip (about 5 g)

Step-by-Step Practical Procedure

  1. Place one nail alone in beaker 1 with salt water (control).
  2. Wrap the second nail tightly with zinc strip, join with copper wire, and place in beaker 2.
  3. Ensure good metal-to-metal contact between zinc and iron.
  4. Leave both for 7 days.
  5. Inspect daily for rust on the iron and white corrosion product on the zinc.
  6. Weigh the zinc strip before and after to estimate metal sacrificed.

Observations & Expected Results

The unprotected nail rusts heavily; the coupled nail stays bright while the zinc develops a white crust of zinc corrosion products and loses mass.

Worked Stoichiometric Calculations

Problem: The zinc strip loses 0.65 g in 7 days. How many moles of electrons did it supply? (Zn = 65.38)

Working: Moles Zn = 0.65/65.38 = 0.00994 mol. Each Zn gives 2e⁻, so electrons = 0.0199 mol ≈ 0.020 mol of electrons.

Safety Precautions & Hazard Control

  • Ensure the wire connections are above the waterline to avoid extra couples.
  • Salt water is low hazard.
  • Dry hands before handling electrical connections if a meter is used.

Waste Disposal Protocol

Salt water down the drain; the zinc strip and nails go in metal recycling.

Viva Voce Oral Defense Questions & Answers

Q: Why is the zinc called 'sacrificial'?

A: It corrodes away (is sacrificed) to keep the iron cathodic and uncorroded.

Q: What happens when all the zinc is consumed?

A: Protection stops and the iron begins to rust — anodes must be replaced.

Q: Name two real applications.

A: Ship hulls, underground pipelines, water heaters, offshore platforms.

← Back to Experiments Directory