CHEMVEN

Alloy Hardening Measured: Scratch Hardness of Copper versus Brass

To quantify solid-solution hardening by comparing the scratch hardness of pure copper with brass and bronze.

Level: UniversitySafety: SafeTime: 40 min
Aim of Experiment: To quantify solid-solution hardening by comparing the scratch hardness of pure copper with brass and bronze.

Theoretical Foundations

In a substitutional solid solution, solute atoms of different size strain the host lattice. Moving dislocations must overcome these strain fields, so the alloy is harder than the pure metal — the basis of solid-solution strengthening. A simple scratch test with a steel point ranks hardness reproducibly enough to show the effect.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Samples: copper strip, brass strip, bronze strip
  • Steel scribe or nail
  • Ruler
  • Magnifying lens
  • Emery paper

Chemical Reagents

  • Copper strip sample
  • Brass strip sample
  • Bronze strip sample

Step-by-Step Practical Procedure

  1. Polish one face of each metal strip with emery paper.
  2. Draw the steel scribe across each strip with the same hand pressure.
  3. Measure the scratch width under the magnifying lens for each metal.
  4. Rank the metals by scratch width (narrower = harder).
  5. Repeat three times and average.
  6. Relate the ranking to the solute content of each alloy.

Observations & Expected Results

Copper shows the widest, deepest scratch; brass is markedly narrower and bronze narrower still, confirming alloy hardening.

Worked Stoichiometric Calculations

Problem: Average scratch widths: Cu 0.42 mm, brass 0.25 mm, bronze 0.18 mm. Express each alloy's hardness relative to copper (hardness ∝ 1/width).

Working: Brass/Cu = 0.42/0.25 = 1.68; bronze/Cu = 0.42/0.18 = 2.33. Brass is about 1.7× and bronze about 2.3× as scratch-hard as copper.

Safety Precautions & Hazard Control

  • Point the scribe away from the body.
  • Secure the strips so they do not slip.
  • No chemicals involved.

Waste Disposal Protocol

No waste; metal strips are reusable.

Viva Voce Oral Defense Questions & Answers

Q: What is solid-solution strengthening?

A: Hardening caused by solute atoms straining the lattice and impeding dislocation motion.

Q: Why is bronze harder than brass here?

A: Tin atoms are larger and less soluble than zinc, giving stronger lattice distortion plus hard phases.

Q: What is a dislocation?

A: A line defect in the crystal lattice whose motion produces plastic deformation.

← Back to Experiments Directory