CHEMVEN

Making Bronze: A Copper-Tin Alloy of the Bronze Age

To prepare a bronze alloy (about 88% Cu, 12% Sn) and compare its properties with copper and brass.

Level: UniversitySafety: Advanced lab onlyTime: 90 min
Aim of Experiment: To prepare a bronze alloy (about 88% Cu, 12% Sn) and compare its properties with copper and brass.

Theoretical Foundations

Bronze is copper alloyed mainly with tin. Tin atoms are larger than copper and have limited solubility, so bronze contains hard intermetallic phases that make it harder and more wear-resistant than brass — the basis of its historical use for tools, weapons, and bearings. Typical density is about 8.7-8.9 g cm⁻³ and the alloy melts around 950-1000 °C.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Furnace or crucible with burner
  • Graphite or clay crucible
  • Crucible tongs
  • Steel mold
  • Balance
  • File
  • Face shield, heat-resistant gloves

Chemical Reagents

  • Copper pieces (about 88 g)
  • Tin pieces (about 12 g)
  • Borax flux (a few grams)

Step-by-Step Practical Procedure

  1. Weigh 88 g of copper and 12 g of tin.
  2. Melt the copper with borax flux.
  3. Stir in the tin, which melts readily (mp 232 °C) and alloys quickly.
  4. Pour into the preheated mold and let cool.
  5. Remove the ingot and file a test face.
  6. Compare color, hardness, and ring (sound) with copper and brass samples.
  7. Measure density by displacement.

Observations & Expected Results

The bronze ingot is reddish-gold, harder and more brittle than brass, and gives a clear ringing tone when struck.

Worked Stoichiometric Calculations

Problem: A 100 g bronze sample contains 12.0 g of tin. What is the mass of copper, and how many moles of tin are present? (Sn = 118.71)

Working: Mass of Cu = 100 − 12.0 = 88.0 g. Moles of Sn = 12.0/118.71 = 0.101 mol.

Safety Precautions & Hazard Control

  • Full heat protection: face shield, gloves, apron, closed shoes.
  • Work in a ventilated area; avoid inhaling metal fumes.
  • Preheat molds and keep all tools dry.
  • Never look directly into the furnace without eye protection.

Waste Disposal Protocol

Collect metal scrap for recycling; cool slag goes in general waste.

Viva Voce Oral Defense Questions & Answers

Q: How does bronze differ compositionally from brass?

A: Bronze is copper + tin; brass is copper + zinc.

Q: Why was bronze historically preferred for tools over pure copper?

A: It is much harder and holds an edge, due to solid-solution and intermetallic hardening.

Q: Why does bronze ring when struck?

A: Its high elastic modulus and low damping transmit sound well — the basis of bell metal.

← Back to Experiments Directory