CHEMVEN

From Density to Atomic Radius: Determining the Radius of Aluminium

To work the unit-cell density equation backwards: find the lattice parameter and metallic radius of fcc aluminium from its measured density.

Level: UniversitySafety: SafeTime: 50 min
Aim of Experiment: To work the unit-cell density equation backwards: find the lattice parameter and metallic radius of fcc aluminium from its measured density.

Theoretical Foundations

Aluminium is fcc (Z = 4) with measured density 2.70 g cm⁻³ and M = 26.98 g mol⁻¹. Rearranging ρ = Z·M/(a³·NA) gives a = (Z·M/(ρ·NA))¹ᐟ³, and in fcc the atoms touch along the face diagonal so r = √2·a/4. The accepted metallic radius of Al is 143 pm.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Calculator
  • Aluminium foil or wire sample
  • Balance
  • Graduated cylinder

Chemical Reagents

  • Aluminium sample (a few grams)
  • Distilled water (for displacement)
  • Detergent (a drop, anti-bubble)

Step-by-Step Practical Procedure

  1. Write the density formula and solve for a: a³ = Z·M/(ρ·NA).
  2. Insert Z = 4, M = 26.98 g mol⁻¹, ρ = 2.70 g cm⁻³, NA = 6.022 × 10²³ mol⁻¹.
  3. Take the cube root to find a in cm, then convert to pm.
  4. Use r = √2·a/4 for the fcc touching direction.
  5. Compare your radius with the literature value 143 pm.
  6. Optionally verify the density by displacement on an aluminium sample.

Observations & Expected Results

The calculation gives a ≈ 405 pm and r ≈ 143 pm, matching the literature metallic radius of aluminium.

Worked Stoichiometric Calculations

Problem: Aluminium is fcc with ρ = 2.70 g cm⁻³ and M = 26.98 g mol⁻¹. Find a and the atomic radius.

Working: a³ = 4 × 26.98/(2.70 × 6.022 × 10²³) = 6.637 × 10⁻²³ cm³, so a = 4.049 × 10⁻⁸ cm = 404.9 pm. r = √2 × 404.9/4 = 143.2 pm.

Safety Precautions & Hazard Control

  • Aluminium is safe to handle.
  • Read volumes at eye level.
  • Keep the balance clean and dry.

Waste Disposal Protocol

No waste; keep the aluminium sample.

Viva Voce Oral Defense Questions & Answers

Q: Why is the touching direction the face diagonal in fcc?

A: Nearest neighbors in fcc are corner-to-face-center atoms, separated by half the face diagonal.

Q: What assumption does this radius calculation make?

A: That atoms are hard spheres touching along the face diagonal.

Q: Would this method work for an alloy? Explain.

A: Only approximately, because an alloy's cell contains atoms of different sizes and the composition must be known.

← Back to Experiments Directory