CHEMVEN

Density from the Unit Cell: Copper and the Face-Centered Cubic Lattice

To determine the theoretical density of copper from its fcc unit cell (a = 361.5 pm) and verify Z = 4 by atom counting.

Level: UniversitySafety: SafeTime: 45 min
Aim of Experiment: To determine the theoretical density of copper from its fcc unit cell (a = 361.5 pm) and verify Z = 4 by atom counting.

Theoretical Foundations

Copper crystallizes in a face-centered cubic lattice: 8 corner atoms shared by 8 cells plus 6 face atoms shared by 2 cells give Z = 8×(1/8) + 6×(1/2) = 4 atoms per cell. With a = 361.5 pm and M = 63.55 g mol⁻¹, the density formula ρ = Z·M/(a³·NA) predicts the familiar 8.96 g cm⁻³.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Calculator
  • Ball-and-stick or sphere-packing model kit
  • Copper wire or strip sample
  • Balance
  • Graduated cylinder

Chemical Reagents

  • Copper metal sample (a short length of wire, a few grams)
  • Distilled water (for displacement)
  • Detergent (a drop, anti-bubble)

Step-by-Step Practical Procedure

  1. Build or sketch the fcc unit cell and count shared atoms to confirm Z = 4.
  2. Convert a = 361.5 pm to 3.615 × 10⁻⁸ cm and cube it.
  3. Apply ρ = Z·M/(a³·NA) with M = 63.55 g mol⁻¹.
  4. Compare with the handbook value 8.96 g cm⁻³.
  5. Weigh the copper sample and find its volume by water displacement.
  6. Compare the measured density with the theoretical value and discuss error sources.

Observations & Expected Results

The calculation gives about 8.93 g cm⁻³, within 0.5% of the handbook value; the displacement measurement agrees within a few percent.

Worked Stoichiometric Calculations

Problem: Calculate the density of copper from a = 361.5 pm, Z = 4, M = 63.55 g mol⁻¹.

Working: a³ = (3.615 × 10⁻⁸)³ = 4.725 × 10⁻²³ cm³. ρ = 4 × 63.55/(4.725 × 10⁻²³ × 6.022 × 10²³) = 254.2/28.45 = 8.93 g cm⁻³.

Safety Precautions & Hazard Control

  • Copper metal is safe to handle; wash hands afterwards.
  • Read the meniscus at eye level in the graduated cylinder.
  • Dry the sample before weighing.

Waste Disposal Protocol

No waste generated; keep the copper sample for reuse.

Viva Voce Oral Defense Questions & Answers

Q: How is Z = 4 obtained for fcc?

A: 8 corners × 1/8 + 6 faces × 1/2 = 1 + 3 = 4.

Q: In fcc, along which direction do atoms touch?

A: The face diagonal: 4r = √2·a.

Q: Why is the measured density slightly lower than theoretical?

A: Surface oxide, trapped air, porosity, or measurement error.

← Back to Experiments Directory