CHEMVEN

Calcium Carbonate in Limestone

To determine calcium carbonate in limestone by back-titration.

Level: UniversitySafety: SafeTime: 60 min
Aim of Experiment: To determine calcium carbonate in limestone by back-titration.

Theoretical Foundations

Limestone is dissolved in a known excess of standard HCl; CaCO3 consumes 2 moles of acid per mole. The residual acid is back-titrated with standard NaOH. 1 mL of 1 N HCl = 50 mg CaCO3. Cement-grade limestone needs over 85% CaCO3 with low magnesia.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Burette
  • Pipette
  • Conical flask
  • Hot plate

Chemical Reagents

  • Limestone powder (0.5 g)
  • 0.5 N hydrochloric acid (50 mL, standardised)
  • 0.5 N sodium hydroxide (standardised)
  • Methyl orange indicator

Step-by-Step Practical Procedure

  1. Weigh 0.5 g limestone into a flask.
  2. Add 50 mL 0.5 N HCl and warm until effervescence stops and the residue is white silica.
  3. Cool and titrate the excess acid with 0.5 N NaOH to methyl orange yellow.
  4. Calculate CaCO3 % = (acid - alkali) x N x 50 x 100 / (weight x 1000).

Observations & Expected Results

Good limestone effervesces vigorously and leaves little residue; titres correspond to 85-98% CaCO3.

Worked Stoichiometric Calculations

Problem: 0.500 g limestone: 50.0 mL of 0.5 N HCl added, back-titrated with 32.0 mL of 0.5 N NaOH. Calculate the CaCO3 percentage.

Working: Acid consumed = 50.0 - 32.0 = 18.0 mL of 0.5 N = 9.0 meq. CaCO3 = 9.0 x 50 = 450 mg = 0.450 g. Percent = 0.450/0.500 x 100 = 90.0%, a cement-grade limestone.

Safety Precautions & Hazard Control

  • Warm gently; violent boiling sprays acid.
  • Ensure complete dissolution of carbonate.
  • Cool before back-titration.
  • Use methyl orange; phenolphthalein gives a fading end point in presence of CO2.

Waste Disposal Protocol

Neutralised solution goes down the drain.

Viva Voce Oral Defense Questions & Answers

Q: Why back-titrate instead of direct titration?

A: Limestone dissolves slowly; the excess-acid method guarantees complete reaction before the residual acid is measured.

Q: Why is magnesia limited in cement limestone?

A: Excess MgO causes unsoundness (delayed expansion) in the finished cement.

← Back to Experiments Directory