CHEMVEN

Manganese in Steel (Bismuthate Method)

To determine manganese in steel by the bismuthate oxidation method.

Level: UniversitySafety: Advanced lab onlyTime: 90 min
Aim of Experiment: To determine manganese in steel by the bismuthate oxidation method.

Theoretical Foundations

Steel is dissolved in nitric acid and Mn2+ is oxidised to purple permanganate by solid sodium bismuthate. After filtering off excess bismuthate, the permanganate is titrated with standard ferrous ammonium sulphate; the end point is the disappearance of pink. 1 mL of 0.1 N FAS = 1.098 mg Mn.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Conical flasks
  • Burette
  • Filter assembly
  • Hot plate

Chemical Reagents

  • Steel sample (1 g)
  • Nitric acid (1:3)
  • Sodium bismuthate (solid)
  • 0.1 N ferrous ammonium sulphate (standardised)
  • Distilled water

Step-by-Step Practical Procedure

  1. Dissolve 1 g steel in nitric acid with heating.
  2. Boil to expel nitrogen oxides, cool slightly.
  3. Add 1 g sodium bismuthate, stir 2 minutes to develop the purple permanganate colour.
  4. Filter through a sintered crucible to remove excess bismuthate.
  5. Titrate immediately with 0.1 N FAS until the pink just disappears.
  6. Calculate Mn % = titre x 0.001098 x 100 / steel weight.

Observations & Expected Results

Plain carbon steel gives a faint pink needing a few mL; Hadfield manganese steel gives an intense purple.

Worked Stoichiometric Calculations

Problem: 1.000 g steel required 7.5 mL of 0.1 N FAS. Calculate the manganese percentage.

Working: Mn = 7.5 x 0.001098 x 100/1.000 = 0.824%. A typical manganese level for carbon steel.

Safety Precautions & Hazard Control

  • Expel all nitrogen oxides; they reduce permanganate.
  • Filter off every trace of bismuthate or it re-oxidises Fe2+.
  • Titrate immediately; permanganate fades on standing.
  • Bismuthate is a strong oxidiser; keep from organics.

Waste Disposal Protocol

Acidic manganese residues go to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is bismuthate used?

A: It is one of the few oxidants strong enough to oxidise Mn2+ fully to MnO4- in nitric acid.

Q: Why must nitrogen oxides be removed?

A: They reduce the formed permanganate back to Mn2+, giving low results.

← Back to Experiments Directory