Analysis of Brass: Copper and Zinc

To determine copper and zinc percentages in a brass sample.

Level: UniversitySafety: Advanced lab onlyTime: 2 h
Aim of Experiment: To determine copper and zinc percentages in a brass sample.

Theoretical Foundations

Brass (Cu-Zn alloy) is dissolved in nitric acid. Copper is determined iodometrically: Cu2+ oxidises KI to iodine, titrated with thiosulphate (1 mL 0.1 N = 6.355 mg Cu). Zinc is then determined by EDTA titration at pH 10 with Eriochrome Black T after masking copper. Typical brass is 60-70% Cu, 30-40% Zn.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Burette
  • Pipettes
  • Conical flasks
  • Volumetric flask

Chemical Reagents

  • Brass turnings (0.5 g)
  • Concentrated nitric acid
  • Potassium iodide
  • 0.1 N sodium thiosulphate
  • 0.01 M EDTA
  • Eriochrome Black T
  • Ammonia buffer (pH 10)

Step-by-Step Practical Procedure

  1. Dissolve 0.5 g brass in nitric acid, evaporate nearly to dryness, and make up to 250 mL.
  2. Copper: pipette 25 mL, neutralise, add KI, and titrate liberated iodine with 0.1 N thiosulphate (starch near end).
  3. Zinc: pipette 25 mL, mask copper with thiosulphate, buffer to pH 10, and titrate with 0.01 M EDTA to blue.
  4. Calculate Cu % = titre x 0.006355 x 10 x 100/0.5 and Zn % = EDTA titre x 0.0006538 x 10 x 100/0.5.

Observations & Expected Results

Cartridge brass gives about 70% Cu and 30% Zn, totalling near 100%.

Worked Stoichiometric Calculations

Problem: 0.500 g brass was made up to 250 mL. A 25 mL aliquot required 5.5 mL of 0.1 N sodium thiosulphate for copper. Calculate the copper percentage.

Working: Cu per aliquot = 5.5 x 6.355 = 34.95 mg. Total Cu = 34.95 x 10 = 349.5 mg = 0.3495 g. Cu % = 0.3495/0.500 x 100 = 69.9%, typical cartridge brass.

Safety Precautions & Hazard Control

  • Remove nitrogen oxides by evaporation or they liberate iodine.
  • Add starch only near the end point.
  • Mask copper fully before the zinc titration.
  • Standardise both titrants.

Waste Disposal Protocol

Copper/zinc residues go to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Write the iodometric copper reaction.

A: 2Cu2+ + 4I- -> 2CuI + I2; the liberated iodine is titrated with thiosulphate.

Q: Why must copper be masked for zinc?

A: Cu2+ also complexes EDTA and the indicator, so it would be counted as zinc.