CHEMVEN

Electroplating of Copper: Verifying Faraday's Laws

To copper-plate a steel object and verify Faraday's first law of electrolysis.

Level: UniversitySafety: Needs supervisionTime: 90 min
Aim of Experiment: To copper-plate a steel object and verify Faraday's first law of electrolysis.

Theoretical Foundations

In acid copper sulphate solution, Cu2+ discharges at the cathode: Cu2+ + 2e- -> Cu. The mass deposited follows Faraday's law: m = (I x t x 63.5) / (2 x 96500). Comparing the weighed deposit with theory gives the cathode current efficiency, the key plating-shop control parameter.

Required Apparatus & Chemicals

Laboratory Apparatus

  • DC power supply
  • Ammeter
  • Copper anode
  • Steel cathode (weighed)
  • Plating bath
  • Stopwatch
  • Balance

Chemical Reagents

  • Acid copper sulphate bath (CuSO4 + H2SO4)
  • Degreasing solution

Step-by-Step Practical Procedure

  1. Degrease and weigh the steel cathode (W1).
  2. Set up the bath with copper anode and steel cathode 5 cm apart.
  3. Pass 1.0 A for 30 minutes, keeping current steady.
  4. Rinse, dry and weigh the cathode (W2).
  5. Calculate theoretical deposit and current efficiency % = actual x 100 / theoretical.
  6. Inspect the deposit for smoothness and adhesion (bend test).

Observations & Expected Results

A bright adherent pink copper layer forms; efficiency is typically 95-100% in acid copper baths.

Worked Stoichiometric Calculations

Problem: 1.0 A for 30 minutes deposited 0.55 g copper. Calculate the theoretical mass and current efficiency.

Working: Theoretical = 1.0 x 1800 x 63.5/(2 x 96500) = 114300/193000 = 0.592 g. Efficiency = 0.55/0.592 x 100 = 92.9%.

Safety Precautions & Hazard Control

  • Degrease thoroughly or the plate peels.
  • Keep current steady; surges give burnt deposits.
  • Do not short the electrodes.
  • Handle the acid bath with gloves and goggles.

Waste Disposal Protocol

Spent copper bath goes to heavy-metal waste, never the drain.

Viva Voce Oral Defense Questions & Answers

Q: State Faraday's first law.

A: The mass of substance deposited is proportional to the quantity of electricity passed: m = Q x equivalent weight / 96500.

Q: Why is sulphuric acid added to the bath?

A: It raises conductivity, prevents Cu(OH)2 precipitation, and improves the deposit's grain structure.

← Back to Experiments Directory