CHEMVEN

Adhesion of Paint: Cross-Hatch Tape Test

To assess paint adhesion by the cross-hatch tape test.

Level: UniversitySafety: SafeTime: 45 min
Aim of Experiment: To assess paint adhesion by the cross-hatch tape test.

Theoretical Foundations

Adhesion is the bond strength between coating and substrate. A lattice of cuts is made through the film to the substrate with a sharp blade; pressure-sensitive tape is applied and pulled off rapidly. The percentage of squares remaining gives an ASTM D3359 rating from 5B (perfect) to 0B (total failure). Good adhesion needs clean, properly prepared surfaces.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Cross-hatch cutter or sharp blade
  • Steel ruler
  • Pressure-sensitive tape
  • Magnifier

Chemical Reagents

  • Painted test panels (on metal and wood, fully cured)

Step-by-Step Practical Procedure

  1. Ensure the paint film is fully cured.
  2. Cut a 6x6 grid of 2 mm squares through the film to the substrate.
  3. Brush off loose flakes.
  4. Press the tape firmly over the lattice and rub down.
  5. Pull the tape off rapidly at 180 degrees.
  6. Count intact squares and assign the ASTM rating (5B = 0% removed, 4B <5%, 3B 5-15%, 2B 15-35%, 1B 35-65%, 0B >65%).

Observations & Expected Results

Well-prepared primed metal scores 5B-4B; paint on greasy or glossy unprepared surfaces scores 1B-0B with large flakes lifting.

Worked Stoichiometric Calculations

Problem: Out of 36 squares, 5 squares lost flakes. Calculate the percent removed and the ASTM rating.

Working: Removed = 5/36 x 100 = 13.9%, which falls in the 5-15% band: rating 3B.

Safety Precautions & Hazard Control

  • Cut fully through to the substrate; shallow cuts give false passes.
  • Use fresh sharp blades for clean cuts.
  • Apply and remove tape with consistent pressure and speed.
  • Test only fully cured films.

Waste Disposal Protocol

Tested panels go to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why does surface preparation matter so much?

A: Grease, rust and glossy old paint prevent the coating wetting and bonding to the substrate, so adhesion fails at the interface.

Q: What is the pull-off test?

A: A quantitative adhesion test where a dolly glued to the coating is pulled until failure, measuring bond strength in MPa.

← Back to Experiments Directory