CHEMVEN

Mordant Dyeing of Wool with Alum

To dye wool with a natural-style mordant dye using alum, comparing mordanted and unmordanted fabric.

Level: UniversitySafety: SafeTime: 90 min
Aim of Experiment: To dye wool with a natural-style mordant dye using alum, comparing mordanted and unmordanted fabric.

Theoretical Foundations

Mordant dyes (e.g. alizarin) have poor affinity alone but form insoluble coloured complexes (lakes) with metal ions fixed on the fibre. Pre-mordanting wool with potash alum deposits Al3+ on the protein chains; the dye then chelates the aluminium, giving deep, fast shades that unmordanted wool cannot hold.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Beakers
  • Water bath
  • Glass rods
  • Balance

Chemical Reagents

  • Wool pieces (5 g each)
  • Potash alum (15% owf)
  • Alizarin or madder dye (5% owf)
  • Cream of tartar (optional assistant)

Step-by-Step Practical Procedure

  1. Mordant one wool piece: simmer 45 minutes in water with 15% owf alum, then rinse.
  2. Prepare the dye bath with alizarin at 5% owf.
  3. Enter both mordanted and unmordanted wool; simmer 45 minutes.
  4. Rinse both in cold water and dry.
  5. Compare colour depth and rub fastness between the two.
  6. Test wash fastness with soap at 50 C.

Observations & Expected Results

Mordanted wool dyes a deep Turkey-red; unmordanted wool takes only a pale pink that washes out.

Worked Stoichiometric Calculations

Problem: 5 g wool needs 15% owf alum. How much alum is required?

Working: 0.15 x 5 = 0.75 g of potash alum.

Safety Precautions & Hazard Control

  • Simmer, do not boil wool or it felts and shrinks.
  • Enter fabric evenly to avoid patchy mordanting.
  • Rinse well; loose dye stains comparisons.
  • Wear gloves when handling hot baths.

Waste Disposal Protocol

Dye baths go to chemical waste.

Viva Voce Oral Defense Questions & Answers

Q: What is a mordant?

A: A metal salt (usually Al, Fe or Cr) that fixes dye to fibre by forming an insoluble dye-metal-fibre complex.

Q: Why does iron mordant darken shades?

A: Iron forms deeply coloured (often black) complexes with the dye, saddening bright reds to maroons and blacks.

← Back to Experiments Directory