Vulcanisation of Rubber (Demo)
To demonstrate sulphur vulcanisation of natural rubber.
Theoretical Foundations
Raw natural rubber is a tacky thermoplastic; heating it with sulphur (2-3%) and accelerators forms sulphur bridges between polyisoprene chains. The crosslinked network becomes elastic, strong and non-tacky: it stretches and recovers instead of flowing. This is the basis of tyres and rubber goods.
Required Apparatus & Chemicals
Laboratory Apparatus
- Two-roll mill or mortar
- Hydraulic press / heated plates
- Oven (140 C)
- Tensile test strips cutter
Chemical Reagents
- Natural rubber (crepe, 50 g)
- Sulphur powder (1.5 g)
- Zinc oxide (2.5 g)
- Accelerator MBTS (0.5 g)
- Stearic acid (1 g)
Step-by-Step Practical Procedure
- Masticate the rubber on the mill and mix in ZnO, stearic acid, accelerator and sulphur uniformly.
- Sheet the compound to 2 mm thickness.
- Cut test strips; keep one strip unvulcanised as control.
- Press-cure the rest at 140 C for 20 minutes.
- Compare: stretch each strip and observe recovery, tackiness and strength.
- Record the qualitative difference vulcanisation makes.
Observations & Expected Results
Uncured rubber stretches permanently and feels tacky; vulcanised rubber snaps back elastically and feels dry.
Worked Stoichiometric Calculations
Problem: The mix uses 1.5 g sulphur per 50 g rubber. Express the sulphur loading in phr (parts per hundred rubber).
Working: phr = 1.5/50 x 100 = 3 phr, a typical soft-rubber vulcanisation loading.
Safety Precautions & Hazard Control
- Keep sulphur dust away from flames.
- Use heat gloves with the press and oven.
- Ensure uniform mixing or cure is patchy.
- Ventilate; accelerators have strong odours.
Waste Disposal Protocol
Rubber trimmings go to solid waste.
Viva Voce Oral Defense Questions & Answers
Q: What does zinc oxide do?
A: It activates the accelerator-sulphur system, speeding cure and improving crosslink efficiency.
Q: What is ebonite?
A: Hard rubber with very high sulphur (25-30%), fully crosslinked into a rigid thermoset used for battery cases.