CHEMVEN

Polystyrene Beads by Suspension Polymerisation

To prepare polystyrene beads by suspension polymerisation of styrene.

Level: UniversitySafety: Needs supervisionTime: 2 h
Aim of Experiment: To prepare polystyrene beads by suspension polymerisation of styrene.

Theoretical Foundations

Styrene monomer is dispersed as droplets in water with a suspending agent (starch or PVA) and polymerised by a monomer-soluble initiator (benzoyl peroxide) at 85 C. Each droplet acts as a mini bulk reactor, giving spherical beads that are easily filtered and washed, the industrial route to expandable polystyrene.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Three-neck flask
  • Reflux condenser
  • Mechanical stirrer
  • Water bath
  • Buchner funnel

Chemical Reagents

  • Styrene (20 mL, freshly distilled)
  • Benzoyl peroxide (0.4 g)
  • Starch solution (1%, 100 mL)
  • Distilled water (100 mL)

Step-by-Step Practical Procedure

  1. Charge the flask with water and starch solution; start stirring at 400 rpm.
  2. Dissolve benzoyl peroxide in styrene and add to the flask.
  3. Heat to 85 C under reflux with continuous stirring for 2 hours.
  4. Cool, filter the beads on a Buchner funnel, and wash with water.
  5. Dry and sieve; record the bead size range and yield.
  6. Test solubility: beads dissolve in toluene but not in water or ethanol.

Observations & Expected Results

White spherical beads 0.5-2 mm form; stirring too slowly gives lumps, too fast gives fines.

Worked Stoichiometric Calculations

Problem: 20 mL styrene (density 0.91 g/mL) gave 15.5 g dry beads. Calculate the percentage conversion.

Working: Monomer mass = 20 x 0.91 = 18.2 g. Conversion = 15.5/18.2 x 100 = 85.2%.

Safety Precautions & Hazard Control

  • Styrene is flammable and its vapours irritate; no open flames.
  • Maintain steady stirring or droplets coalesce.
  • Keep at 85 C; higher temperatures cause runaway.
  • Benzoyl peroxide is an oxidiser; keep away from heat when dry.

Waste Disposal Protocol

Filtrate goes to aqueous organic waste; beads are solid waste.

Viva Voce Oral Defense Questions & Answers

Q: What is the role of starch?

A: It is a suspending agent that stabilises monomer droplets and prevents them coalescing during polymerisation.

Q: Why is suspension preferred over bulk polymerisation?

A: Water absorbs the reaction heat, preventing runaway, and the bead product is easy to handle.

← Back to Experiments Directory