Preparation of Bakelite (Phenol-Formaldehyde Resin)

To prepare bakelite resin from phenol and formaldehyde.

Level: UniversitySafety: Needs supervisionTime: 90 min
Aim of Experiment: To prepare bakelite resin from phenol and formaldehyde.

Theoretical Foundations

Phenol condenses with formaldehyde under acid or alkaline catalysis to give a resol that crosslinks on heating into an infusible thermoset (bakelite). The three-dimensional methylene-bridged network makes it hard, heat-resistant and electrically insulating, the classic material for switches and handles.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Round-bottom flask
  • Reflux condenser
  • Water bath
  • Beaker
  • Glass rod

Chemical Reagents

  • Phenol (10 g, melted)
  • Formalin (15 mL, 40%)
  • Concentrated hydrochloric acid (2 mL, catalyst)
  • Distilled water

Step-by-Step Practical Procedure

  1. Mix melted phenol and formalin in the flask and add the acid catalyst.
  2. Reflux gently on a water bath for 30-45 minutes until a viscous pink resin separates.
  3. Pour off the aqueous layer and wash the resin with warm water.
  4. Transfer the resin to a beaker and heat on the water bath to drive off water.
  5. Pour into a mould and cure at 100 C until hard and infusible.
  6. Test hardness and insolubility of the cured product.

Observations & Expected Results

The mixture turns pink and thickens; curing gives a hard, brown, glossy solid that cannot be remelted.

Worked Stoichiometric Calculations

Problem: 10.0 g phenol (M = 94) with excess formaldehyde gave 11.5 g cured resin. If each phenol adds one CH2 bridge (net +12 mass per phenol), calculate the theoretical mass and yield.

Working: Moles phenol = 10/94 = 0.1064. Theoretical = 0.1064 x 106 = 11.28 g. Yield = 11.5/11.28 x 100 = 102% (slightly over, indicating trapped water; dry further).

Safety Precautions & Hazard Control

  • Phenol is corrosive and toxic; wear gloves and goggles.
  • Formalin vapours irritate; work in a fume cupboard.
  • Control reflux; the reaction is exothermic and can surge.
  • Do not overheat the curing resin or it chars.

Waste Disposal Protocol

Aqueous waste goes to chemical waste; cured resin is solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is bakelite a thermoset?

A: Its phenol rings are linked by methylene bridges into a 3D crosslinked network that cannot flow on reheating.

Q: What is the difference between novolac and resol?

A: Novolac (acid catalyst, excess phenol) is linear and needs a hardener; resol (alkaline, excess formaldehyde) crosslinks on heating alone.

← Back to Experiments Directory