Nylon 6,6 by Interfacial Polymerisation
To prepare nylon 6,6 at a liquid-liquid interface and draw it as a fibre.
Theoretical Foundations
Hexamethylenediamine in water reacts with adipoyl chloride in an immiscible organic solvent at their interface, forming polyamide film instantly (condensation polymerisation with HCl eliminated). Because the polymer forms only at the interface, it can be continuously pulled out as a rope, demonstrating the 'nylon rope trick'.
Required Apparatus & Chemicals
Laboratory Apparatus
- Beaker (250 mL)
- Glass rod / forceps
- Measuring cylinders
Chemical Reagents
- Hexamethylenediamine solution (5% aqueous, 50 mL)
- Adipoyl chloride solution (5% in hexane, 50 mL)
- Sodium hydroxide (to neutralise HCl)
Step-by-Step Practical Procedure
- Pour 50 mL hexamethylenediamine solution into the beaker.
- Carefully layer 50 mL adipoyl chloride solution down the wall so the liquids do not mix.
- Wait 30 seconds for a white polymer film to form at the interface.
- Grip the film with forceps and pull steadily upward, winding the continuous rope on a glass rod.
- Rinse the rope with water and dry.
- Weigh the dried nylon and note its toughness.
Observations & Expected Results
A tough white rope several metres long can be drawn; the interface reforms film continuously until monomers exhaust.
Worked Stoichiometric Calculations
Problem: 0.50 g hexamethylenediamine (M = 116) reacted with excess adipoyl chloride (M = 183) to give 0.80 g nylon 6,6 (repeat unit M = 226). Calculate the percentage yield.
Working: Moles diamine = 0.50/116 = 0.00431. Theoretical nylon = 0.00431 x 226 = 0.974 g. Yield = 0.80/0.974 x 100 = 82.1%.
Safety Precautions & Hazard Control
- Adipoyl chloride is a lachrymator; handle in a fume cupboard with gloves.
- Layer the solutions gently; mixing gives lumps instead of film.
- Pull slowly and steadily for a continuous rope.
- Wash hands after handling monomers.
Waste Disposal Protocol
Unreacted monomer solutions go to organic chemical waste; the nylon rope is solid waste.
Viva Voce Oral Defense Questions & Answers
Q: Why is it called 6,6 nylon?
A: Both monomers (hexamethylenediamine and adipic acid derivative) contain 6 carbon atoms.
Q: Why does the polymer form only at the interface?
A: The monomers are in immiscible phases and meet only at the boundary, so reaction is confined there.