CHEMVEN

Proximate Analysis of Coal: Moisture

To determine the moisture content of a coal sample (proximate analysis, part 1).

Level: UniversitySafety: SafeTime: 2 h
Aim of Experiment: To determine the moisture content of a coal sample (proximate analysis, part 1).

Theoretical Foundations

Moisture in coal is useless weight that evaporates in the furnace, lowering the effective calorific value and causing handling problems. Heating 1 g of air-dried coal at 105-110 C to constant weight drives off moisture; the loss gives the moisture percentage, the first of the four proximate parameters.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Hot air oven (108 C)
  • Weighing bottles with lids
  • Desiccator
  • Analytical balance

Chemical Reagents

  • Coal sample (1 g, 72-mesh, air-dried)

Step-by-Step Practical Procedure

  1. Weigh 1 g coal into a tared weighing bottle.
  2. Heat uncovered at 105-110 C for 1 hour.
  3. Cover, cool in a desiccator, and weigh.
  4. Repeat heating for 30 minutes until constant weight.
  5. Calculate moisture % = loss x 100 / sample weight.

Observations & Expected Results

Air-dried bituminous coal shows 1-5% moisture; lignite may exceed 20%.

Worked Stoichiometric Calculations

Problem: 1.000 g coal weighed 0.972 g after drying. Calculate the moisture content.

Working: Moisture = (1.000 - 0.972)/1.000 x 100 = 2.8%.

Safety Precautions & Hazard Control

  • Use the specified 105-110 C range; higher temperatures oxidise the coal.
  • Cover the bottle before removing from the oven.
  • Cool in a desiccator; hot coal reabsorbs moisture.
  • Grind to the specified fineness for representative drying.

Waste Disposal Protocol

Dried coal goes to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: What is the difference between surface and inherent moisture?

A: Surface moisture comes from rain/washing and is easily removed; inherent moisture is held in pores and needs oven drying.

Q: How does moisture affect coal price?

A: Buyers pay for dry coal; high moisture means paying for water and getting less heat.

← Back to Experiments Directory