CHEMVEN

Silica and Insoluble Residue in Cement

To estimate silica and insoluble residue in ordinary Portland cement.

Level: UniversitySafety: Advanced lab onlyTime: 3 h
Aim of Experiment: To estimate silica and insoluble residue in ordinary Portland cement.

Theoretical Foundations

Cement is dissolved in HCl; silica is dehydrated by evaporation and weighed as SiO2 after ignition. The insoluble residue (unreactive silica, measured after Na2CO3 digestion of the soluble part) must not exceed 2-4% in OPC. High residue indicates adulteration with sand or poor-quality raw mix.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Beakers
  • Water bath
  • Filter paper (ashless)
  • Muffle furnace
  • Analytical balance

Chemical Reagents

  • Cement (1 g)
  • Concentrated hydrochloric acid
  • Sodium carbonate solution
  • Distilled water

Step-by-Step Practical Procedure

  1. Dissolve 1 g cement in dilute HCl with warming.
  2. Evaporate to dryness on a water bath to dehydrate silica; bake 1 hour.
  3. Re-dissolve soluble salts in dilute HCl and filter through ashless paper.
  4. Wash, ignite the residue at 1000 C and weigh as crude silica.
  5. Treat a separate portion with hot sodium carbonate, filter, ignite and weigh the insoluble residue.
  6. Calculate percentages on the cement weight.

Observations & Expected Results

OPC shows 20-25% silica and under 2% insoluble residue; sandy adulteration raises the residue sharply.

Worked Stoichiometric Calculations

Problem: 1.000 g cement gave 0.225 g ignited silica and 0.015 g insoluble residue. Report both percentages.

Working: Silica = 22.5%; insoluble residue = 1.5%. Both within normal OPC ranges.

Safety Precautions & Hazard Control

  • Bake the dried residue thoroughly; incomplete dehydration loses silica to the filtrate.
  • Use ashless filter paper and correct for its ash.
  • Handle concentrated HCl in a fume cupboard.
  • Ignite to constant weight at 1000 C.

Waste Disposal Protocol

Acid filtrates are neutralised before disposal; ignited residues go to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is the solution evaporated to dryness?

A: To dehydrate silicic acid into insoluble SiO2 so it is fully retained on the filter.

Q: What does high insoluble residue indicate?

A: Contamination with sand, clay or other inert material, or adulteration of the cement.

← Back to Experiments Directory