CHEMVEN

Loss on Ignition of Cement

To determine the loss on ignition (LOI) of a cement sample.

Level: UniversitySafety: Needs supervisionTime: 2 h
Aim of Experiment: To determine the loss on ignition (LOI) of a cement sample.

Theoretical Foundations

LOI measures volatile constituents (combined water, CO2 from carbonation, organic matter) driven off at 900-1000 C. Fresh OPC has LOI under 4-5%; high LOI indicates the cement has absorbed moisture and CO2 during bad storage (pre-hydration and carbonation), which reduces its strength potential.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Muffle furnace (1000 C)
  • Platinum or silica crucible
  • Desiccator
  • Analytical balance
  • Tongs

Chemical Reagents

  • Cement sample (1 g, dried)

Step-by-Step Practical Procedure

  1. Weigh 1 g cement into a tared crucible.
  2. Ignite in the muffle furnace at 950 C for 1 hour.
  3. Cool in a desiccator and weigh.
  4. Repeat ignition to constant weight.
  5. Calculate LOI % = loss x 100 / sample weight.

Observations & Expected Results

Fresh cement loses 1-3%; weathered cement may lose over 8% and feels lumpy.

Worked Stoichiometric Calculations

Problem: 1.000 g cement weighed 0.958 g after ignition. Calculate the LOI and comment.

Working: LOI = (1.000 - 0.958)/1.000 x 100 = 4.2%. Just within the usual 5% limit, but the cement should be used promptly.

Safety Precautions & Hazard Control

  • Handle the hot crucible only with tongs.
  • Cool fully in a desiccator before weighing.
  • Ignite to constant weight.
  • Keep the furnace ventilated; CO2 evolves during ignition.

Waste Disposal Protocol

Ignited residue goes to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: What gases are lost during ignition?

A: Water from pre-hydrated compounds and carbon dioxide from carbonated lime.

Q: Why does high LOI mean weak cement?

A: It shows part of the cement already reacted with air moisture, leaving less active clinker to hydrate in concrete.

← Back to Experiments Directory