Complete Analysis of Brass: Copper by Iodometry, Zinc by EDTA

To determine both Cu and Zn in brass by a combined iodometric-complexometric scheme.

Level: UniversitySafety: Advanced lab onlyTime: 3 h
Aim of Experiment: To determine both Cu and Zn in brass by a combined iodometric-complexometric scheme.

Theoretical Foundations

Brass (Cu-Zn) is dissolved in HNO3 and made to 250.0 mL. Aliquot A: Cu2+ by iodometry (2Cu2+ + 4I- -> 2CuI + I2; 1 Cu = 1 S2O3(2-)). Aliquot B: (Cu2+ + Zn2+) by EDTA at pH 10 (EBT); Zn = total - Cu. This capstone combines precipitation-free redox and complexometric titrations on one sample.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 50 mL burette
  • 250 mL volumetric flask
  • 25 mL pipettes
  • 250 mL iodine flask
  • 250 mL conical flask
  • Analytical balance
  • Fume cupboard

Chemical Reagents

  • Brass sample
  • Conc. HNO3 + conc. H2SO4 (dissolution/fuming)
  • KI crystals
  • Standardised Na2S2O3 (0.1000 M)
  • Standardised EDTA (0.1000 M)
  • pH 10 buffer
  • Eriochrome Black T
  • Starch indicator

Step-by-Step Practical Procedure

  1. Weigh about 1.000 g brass; dissolve in HNO3 in a fume cupboard; fume off with H2SO4; make up to 250.0 mL.
  2. Aliquot A (25.00 mL): add KI, titrate I2 with 0.1000 M thiosulfate (starch) for Cu.
  3. Aliquot B (25.00 mL): add pH 10 buffer and EBT; titrate with 0.1000 M EDTA for Cu + Zn.
  4. Zn-EDTA volume = V(EDTA) - V(thio) x (M(thio)/M(EDTA)).
  5. Calculate % Cu and % Zn (M: Cu 63.55, Zn 65.38).

Observations & Expected Results

Iodometry: blue to white endpoint, about 10.23 mL. EDTA: wine-red to blue, about 14.35 mL.

Worked Stoichiometric Calculations

Problem: 1.000 g brass to 250.0 mL. Aliquot A: 10.23 mL of 0.1000 M thiosulfate. Aliquot B: 14.35 mL of 0.1000 M EDTA. Find % Cu and % Zn.

Working: Cu: moles = 0.1000 x 0.01023 = 0.0010230 mol in 25 mL; total 0.010230 mol; mass = 0.010230 x 63.55 = 0.65012 g; % Cu = 65.0%. Total metal EDTA = 0.1000 x 0.01435 = 0.0014350 mol; Zn = 0.0014350 - 0.0010230 = 0.00041200 mol in 25 mL; total 0.0041200 mol; mass = 0.0041200 x 65.38 = 0.26937 g; % Zn = 26.9%. Sum 91.9% (balance Pb, Sn, Fe).

Safety Precautions & Hazard Control

  • Remove all HNO3/HNO2 before iodometry.
  • Fume-cupboard dissolution only.
  • Use the same dilution for both aliquots.

Waste Disposal Protocol

Copper/zinc/iodide waste to heavy-metal aqueous waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is Zn found by difference rather than directly?

A: No indicator is selective for Zn2+ in the presence of Cu2+ under simple conditions; Cu is measured selectively by iodometry and subtracted.

Q: What assumption does the difference method make?

A: That Cu and Zn are the only EDTA-consuming metals present; Pb, Fe or Al would inflate the apparent zinc.

← Back to Experiments Directory