CHEMVEN

Silver in a Coin Alloy: Volhard Direct Titration

To determine % Ag in a silver coin alloy by direct Volhard titration.

Level: UniversitySafety: Advanced lab onlyTime: 90 min
Aim of Experiment: To determine % Ag in a silver coin alloy by direct Volhard titration.

Theoretical Foundations

The alloy is dissolved in HNO3: 3Ag + 4HNO3 -> 3AgNO3 + NO + 2H2O. Ag+ is titrated directly with standard SCN-: Ag+ + SCN- -> AgSCN(s); Fe3+ indicator gives red FeSCN(2+) at the first excess. Cu2+ (blue) is present but does not interfere if the red endpoint is read carefully.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 50 mL burette
  • 250 mL volumetric flask
  • 25 mL pipette
  • 250 mL conical flask
  • Analytical balance
  • Fume cupboard

Chemical Reagents

  • Silver coin (about 1 g)
  • Conc. HNO3
  • Standard KSCN (0.1000 M)
  • Ferric ammonium sulfate indicator
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh about 1.000 g coin; dissolve in 10 mL conc. HNO3 in a fume cupboard.
  2. Boil off nitrogen oxides; cool; make up to 250.0 mL.
  3. Pipette 25.00 mL into a flask; add Fe3+ indicator.
  4. Titrate with 0.1000 M SCN- to the first permanent red-brown.
  5. Calculate % Ag (M = 107.87).

Observations & Expected Results

Blue Cu2+ solution; white AgSCN precipitates; red endpoint. Typical titre about 8.34 mL.

Worked Stoichiometric Calculations

Problem: 1.000 g coin to 250.0 mL; 25.00 mL aliquot needed 8.34 mL of 0.1000 M SCN-. Find % Ag.

Working: Moles SCN- = 0.1000 x 0.00834 = 0.00083400 mol = moles Ag+ in aliquot. In 250 mL: 0.0083400 mol. Mass = 0.0083400 x 107.87 = 0.89964 g. % = 90.0% Ag.

Safety Precautions & Hazard Control

  • Dissolve in HNO3 only in a fume cupboard (NOx fumes).
  • Boil off all nitrogen oxides; HNO2 oxidises SCN-.
  • Cu2+ blue colour: read the red endpoint against white.

Waste Disposal Protocol

Silver/copper acidic waste to heavy-metal waste; recover silver if possible.

Viva Voce Oral Defense Questions & Answers

Q: Why must nitrogen oxides be boiled off?

A: HNO2 oxidises thiocyanate, consuming SCN- and giving a falsely high silver titre.

Q: Does the copper in the coin interfere?

A: No: Cu2+ does not precipitate with SCN- under these conditions; it only colours the solution blue.

← Back to Experiments Directory