Zinc by EDTA: Xylenol Orange at pH 5.5

To determine zinc in a brass sample by EDTA titration with xylenol orange.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To determine zinc in a brass sample by EDTA titration with xylenol orange.

Theoretical Foundations

Zn2+ forms a stable EDTA complex even at pH 5-6 (log K = 16.5), where many interferences are weaker. Xylenol orange is red as the Zn complex and yellow when free: Zn2+ + H2Y(2-) -> ZnY(2-) + 2H+. Hexamine buffer holds pH 5.5. Cu2+ would interfere and is masked or absent here after separation.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 50 mL burette
  • 25 mL pipette
  • 250 mL volumetric flask
  • 250 mL conical flask
  • Analytical balance
  • Fume cupboard

Chemical Reagents

  • Brass sample
  • Dilute HNO3
  • Standardised EDTA (0.01004 M)
  • Hexamine buffer (pH 5.5)
  • Xylenol orange indicator
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh about 0.5000 g brass; dissolve in dilute HNO3 in a fume cupboard; make up to 250.0 mL.
  2. Pipette 25.00 mL into a flask.
  3. Add hexamine buffer to pH 5.5.
  4. Add 3 drops xylenol orange (red).
  5. Titrate with 0.01004 M EDTA to pure yellow.
  6. Calculate % Zn (M = 65.38).

Observations & Expected Results

Red to yellow endpoint. Typical titre about 15.20 mL.

Worked Stoichiometric Calculations

Problem: 0.5000 g brass to 250.0 mL; 25.00 mL aliquot needed 15.20 mL of 0.01004 M EDTA. Find % Zn.

Working: Moles EDTA = 0.01004 x 0.01520 = 0.00015261 mol = moles Zn2+ in aliquot. In 250 mL: 0.0015261 mol. Mass = 0.0015261 x 65.38 = 0.099776 g. % = 0.099776/0.5000 x 100 = 20.0%.

Safety Precautions & Hazard Control

  • Control pH at 5-6; outside this the indicator fails.
  • Remove/allow for Cu2+, which also complexes.
  • Dissolve metals only in a fume cupboard.

Waste Disposal Protocol

Zinc/copper acidic waste to heavy-metal aqueous waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is pH 5.5 chosen for zinc?

A: ZnY(2-) is stable enough (log K' still large) while protonation of EDTA suppresses weaker metal complexes, improving selectivity.

Q: What colour change does xylenol orange show?

A: Red (metal-indicator complex) to yellow (free indicator) at the endpoint.