CHEMVEN

Manganese in Steel: Persulfate Oxidation, Arsenite Titration

To determine % Mn in steel by oxidation to permanganate and titration with standard arsenite.

Level: UniversitySafety: Advanced lab onlyTime: 2 h
Aim of Experiment: To determine % Mn in steel by oxidation to permanganate and titration with standard arsenite.

Theoretical Foundations

Persulfate with Ag+ catalyst oxidises Mn2+ to MnO4(-): 2Mn2+ + 5S2O8(2-) + 8H2O -> 2MnO4(-) + 10SO4(2-) + 16H+. Boiling destroys excess persulfate. Titration: 2MnO4(-) + 5AsO3(3-) + 6H+ -> 2Mn2+ + 5AsO4(3-) + 3H2O (sodium arsenite, standardised against KBrO3).

Required Apparatus & Chemicals

Laboratory Apparatus

  • 50 mL burette
  • 250 mL conical flask
  • 250 mL volumetric flask
  • Bunsen burner
  • Analytical balance
  • Fume cupboard

Chemical Reagents

  • Steel drillings
  • Dilute H2SO4 / HNO3
  • Ammonium persulfate
  • AgNO3 catalyst
  • Standard Na3AsO3 (0.05000 M)
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh about 1.000 g steel; dissolve in dilute H2SO4/HNO3 in a fume cupboard.
  2. Add AgNO3 and persulfate; boil 2 min to develop the purple MnO4(-).
  3. Boil a further 5 min to destroy excess persulfate; cool.
  4. Make up to 250.0 mL.
  5. Pipette 25.00 mL; titrate with 0.05000 M arsenite to colourless.
  6. Calculate % Mn (M = 54.94).

Observations & Expected Results

Purple permanganate colour develops; titration to colourless. Typical titre about 0.86 mL of 0.05000 M arsenite (10 mL microburette).

Worked Stoichiometric Calculations

Problem: 1.000 g steel to 250.0 mL; 25.00 mL aliquot needed 0.86 mL of 0.05000 M arsenite. Find % Mn (M = 54.94).

Working: Moles AsO3(3-) = 0.05000 x 0.00086 = 0.000043000 mol. Moles MnO4(-) = 0.000043000 x 2/5 = 0.000017200 mol = moles Mn in aliquot. In 250 mL: 0.00017200 mol. Mass = 0.00017200 x 54.94 = 0.0094497 g. % = 0.0094497/1.000 x 100 = 0.945% Mn.

Safety Precautions & Hazard Control

  • Arsenite is toxic: gloves, no mouth pipetting, dedicated waste.
  • Destroy excess persulfate completely or it oxidises arsenite.
  • Chloride must be absent (forms Cl2 with persulfate).

Waste Disposal Protocol

Arsenic waste is highly toxic: collect separately in labelled arsenic waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is Ag+ added?

A: Ag+ catalyses persulfate oxidation of Mn2+ to MnO4(-); without it the oxidation is slow and incomplete.

Q: Why must excess persulfate be boiled off?

A: Residual S2O8(2-) would oxidise the arsenite titrant, giving a falsely high manganese result.

← Back to Experiments Directory