Theoretical Foundations
Brass is dissolved in HNO3, fumed with H2SO4 to remove nitrate, then: 2Cu2+ + 4I- -> 2CuI(s) + I2. Liberated iodine is titrated with standard thiosulfate (starch near endpoint). 1 Cu2+ = 1 S2O3(2-). Zn2+ does not interfere.
Required Apparatus & Chemicals
Laboratory Apparatus
- 50 mL burette
- 250 mL volumetric flask
- 250 mL iodine flask
- Analytical balance
- Fume cupboard
- Bunsen burner
Chemical Reagents
- Brass turnings
- Conc. HNO3
- Conc. H2SO4
- KI crystals
- Standardised Na2S2O3 (0.1000 M)
- Starch indicator
- NH4HF2 or urea (nitrite removal, optional)
Step-by-Step Practical Procedure
- Weigh about 1.000 g brass; dissolve in 10 mL conc. HNO3 in a fume cupboard.
- Add 5 mL conc. H2SO4; fume to remove all HNO3; cool and dilute.
- Make up to 250.0 mL.
- Pipette 25.00 mL into an iodine flask; neutralise excess acid with NH3 to faint turbidity, re-acidify slightly.
- Add 2 g KI; titrate with 0.1000 M thiosulfate, starch near the end, to disappearance of blue.
- Calculate % Cu (M = 63.55).
Observations & Expected Results
Brown I2 liberated; creamy CuI precipitate; starch-blue to white endpoint. Typical titre about 10.23 mL.
Worked Stoichiometric Calculations
Problem: 1.000 g brass to 250.0 mL; 25.00 mL aliquot needed 10.23 mL of 0.1000 M thiosulfate. Find % Cu.
Working: Moles thio = 0.1000 x 0.01023 = 0.0010230 mol. Moles I2 = half = 0.00051150 mol. Moles Cu2+ = 2 x 0.00051150 = 0.0010230 mol in aliquot. In 250 mL: 0.010230 mol. Mass Cu = 0.010230 x 63.55 = 0.6501 g. % = 65.0%.
Safety Precautions & Hazard Control
- Remove all HNO3/HNO2; nitrite oxidises I- and inflates the titre.
- Keep pH 3-4; strongly acidic media cause air-oxidation of I-.
- Dissolve metals only in a fume cupboard.
Waste Disposal Protocol
Copper/iodide waste to heavy-metal aqueous waste.
Viva Voce Oral Defense Questions & Answers
Q: Why must nitrate be removed before adding KI?
A: HNO2/NOx oxidise iodide to iodine, liberating extra I2 and giving a falsely high copper result.
Q: Why does the reaction go to completion despite I2 being an oxidant?
A: CuI precipitates, removing Cu+ and driving the equilibrium 2Cu2+ + 4I- -> 2CuI + I2 to the right.