Iron in Haematite Ore: Dichromate after Tin(II) Reduction

To determine % Fe in haematite ore by reduction with SnCl2 and titration with standard K2Cr2O7.

Level: UniversitySafety: Advanced lab onlyTime: 2 h
Aim of Experiment: To determine % Fe in haematite ore by reduction with SnCl2 and titration with standard K2Cr2O7.

Theoretical Foundations

Ore Fe(III) is dissolved in HCl and reduced: 2Fe3+ + Sn2+ -> 2Fe2+ + Sn4+. Excess Sn2+ is removed with HgCl2 (silky white Hg2Cl2 precipitate proves slight excess). Then: Cr2O7(2-) + 6Fe2+ + 14H+ -> 2Cr3+ + 6Fe3+ + 7H2O, using diphenylamine sulfonate indicator (violet endpoint). Dichromate is a primary standard.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 50 mL burette
  • 250 mL conical flask
  • 250 mL volumetric flask
  • Bunsen burner
  • Analytical balance
  • Fume cupboard

Chemical Reagents

  • Haematite ore (powdered)
  • Conc. HCl
  • SnCl2 solution
  • HgCl2 solution (saturated)
  • Standard K2Cr2O7 (0.01667 M)
  • Diphenylamine sulfonate indicator
  • H3PO4 (to complex Fe3+)

Step-by-Step Practical Procedure

  1. Weigh about 1.000 g ore; dissolve in 20 mL conc. HCl with heating in a fume cupboard.
  2. Dilute, heat to boiling, add SnCl2 dropwise until the yellow Fe3+ colour just disappears, plus 2 drops excess.
  3. Cool rapidly; add 10 mL saturated HgCl2; wait 5 min for the silky white precipitate.
  4. Dilute to 250.0 mL.
  5. Pipette 25.00 mL; add H3PO4 and indicator; titrate with K2Cr2O7 to the violet endpoint.
  6. Calculate % Fe.

Observations & Expected Results

Yellow solution goes colourless on reduction; white Hg2Cl2 confirms slight Sn2+ excess; titration goes green to intense violet. Typical titre about 11.64 mL.

Worked Stoichiometric Calculations

Problem: 1.000 g ore to 250.0 mL; 25.00 mL aliquot needed 11.64 mL of 0.01667 M K2Cr2O7. Find % Fe (M = 55.85).

Working: Moles Cr2O7(2-) = 0.01667 x 0.01164 = 0.00019404 mol. Moles Fe2+ in aliquot = 6 x 0.00019404 = 0.00116424 mol. In 250 mL: 0.0116424 mol. Mass Fe = 0.0116424 x 55.85 = 0.6502 g. % = 65.0%.

Safety Precautions & Hazard Control

  • HgCl2 is highly toxic: gloves, no skin contact, collect all mercury waste.
  • SnCl2 excess must be slight; a large excess gives grey metallic Hg and a high result.
  • Dissolve ore in a fume cupboard (HCl fumes).

Waste Disposal Protocol

All mercury-containing residues go to the dedicated mercury waste container, never the sink.

Viva Voce Oral Defense Questions & Answers

Q: What does the white precipitate prove?

A: That a slight excess of Sn2+ was present (reduced to white Hg2Cl2); no precipitate means incomplete reduction, grey Hg means too much Sn2+.

Q: Why is H3PO4 added before titration?

A: It complexes Fe3+ as colourless [Fe(HPO4)]+, removing the yellow colour that would mask the indicator and lowering the Fe3+/Fe2+ potential.