Spectrophotometric Determination of Nickel in Alloy Steel using Dimethylglyoxime
To determine trace to minor amounts of nickel in an alloy steel sample by oxidation of nickel(II) to nickel(IV) with bromine water and formation of the wine-red soluble bis(dimethylglyoximato)nickel(IV) complex in alkaline medium at 445 nm.
Theoretical Foundations
In classical gravimetric analysis, nickel(II) reacts with dimethylglyoxime (dmgH2) in neutral-to-ammoniacal medium to precipitate insoluble scarlet-red [Ni(dmgH)2]. However, when nickel is first treated with a strong oxidising agent (such as saturated bromine water, iodine, or persulphate) in alkaline medium before adding dimethylglyoxime, nickel(II) is oxidised to nickel(IV), forming a brilliant wine-red, water-soluble coordination complex: Ni2+ + Br2 + 2OH- -> Ni(IV) + 2Br- + 2H2O; Ni(IV) + 2(dmgH2) + 4OH- -> [Ni(dmg)2]2- + 4H2O. This oxidized complex remains completely in solution and exhibits a strong absorption maximum at 445 nm (epsilon ≈ 15,000 L·mol^-1·cm^-1), providing a sensitive method for measuring 0.5 to 10 mg/L Ni.
Required Apparatus & Chemicals
Laboratory Apparatus
- Visible spectrophotometer (380-700 nm)
- Matched 1.00 cm cuvettes
- 100 mL volumetric flasks (six)
- 10 mL volumetric pipettes
- Fume cupboard
- Analytical balance (±0.0001 g)
Chemical Reagents
- Standard nickel stock solution (100 mg/L Ni from NiSO4·6H2O)
- Saturated bromine water (Caution: Fume hood)
- Concentrated aqueous ammonia (15 M NH3)
- Dimethylglyoxime solution (1% w/v in 95% ethanol)
- Citric acid or sodium tartrate (20% w/v, masking agent for Fe/Al)
- Deionised water
Step-by-Step Practical Procedure
- Pipette 0.00 (blank), 1.00, 2.00, 4.00, 6.00, and 8.00 mL of 10.0 mg/L Ni standard into separate 100 mL volumetric flasks.
- Pipette 5.00 mL of the prepared unknown steel digest into another 100 mL volumetric flask.
- To each flask, add 5.0 mL of 20% citric acid solution to mask iron and aluminium.
- Add 2.0 mL of saturated bromine water inside a fume hood; swirl and allow 1-2 minutes for oxidation (yellow-brown bromine color persists).
- Add concentrated aqueous ammonia dropwise with swirling until the bromine color is completely discharged, then add 5.0 mL excess ammonia (solution becomes alkaline, pH ~10.5).
- Add 3.0 mL of 1% ethanolic dimethylglyoxime solution; swirl thoroughly. A wine-red color develops immediately.
- Dilute each flask to the 100.0 mL mark with deionised water, stopper, and mix.
- Allow 10 minutes for full color maturation; the complex is stable for at least 1 hour.
- Zero the spectrophotometer with the reagent blank at 445 nm, measure absorbance of standards and sample, and construct the calibration graph to determine nickel concentration.
Observations & Expected Results
Addition of bromine water gives an amber color. Ammonia discharges the bromine and produces a pale alkaline mixture. Addition of DMG triggers an immediate transformation into a sparkling wine-red homogeneous solution. Absorbance is strictly proportional to nickel concentration across 0.1 to 5.0 mg/L Ni.
Worked Stoichiometric Calculations
Problem: 0.2500 g of alloy steel was dissolved and diluted to 250.0 mL. A 5.00 mL aliquot was oxidized, treated with DMG, and diluted to 100.0 mL, giving A = 0.365 at 445 nm. Calibration curve: A = 0.245 × C (mg/L Ni). Calculate the percentage of nickel in the steel.
Working: Concentration in measured flask C = 0.365 / 0.245 = 1.490 mg/L Ni. Mass of Ni in 100 mL flask = 1.490 mg/L × 0.100 L = 0.1490 mg Ni. Aliquot factor = 250.0 mL / 5.00 mL = 50. Total mass of Ni in steel sample = 0.1490 mg × 50 = 7.450 mg = 0.007450 g Ni. Percentage Ni in steel = (0.007450 g / 0.2500 g) × 100 = 2.98% Ni.
Safety Precautions & Hazard Control
- Dispense saturated bromine water exclusively in a fume cupboard; avoid inhaling toxic Br2 vapors.
- Citric acid or tartaric acid must be added before ammonia to prevent precipitation of iron(III) hydroxide.
Waste Disposal Protocol
Bromine and nickel waste must be deactivated with sodium thiosulphate and collected in heavy metal toxic waste.
Viva Voce Oral Defense Questions & Answers
Q: How does the spectrophotometric nickel-DMG complex differ from the gravimetric precipitate?
A: In gravimetric analysis, nickel is in the +2 oxidation state and forms an insoluble scarlet-red precipitate [Ni(dmgH)2]. In spectrophotometry, an oxidising agent (Br2) oxidises nickel to the +4 (or +3) oxidation state in alkaline medium, yielding a soluble, intensely wine-red coordination complex.
Q: Why is citric acid or tartaric acid added before ammonia?
A: Iron(III) present in steel hydrolyses in alkaline ammonia to form a dense reddish-brown gelatinous precipitate of Fe(OH)3 which obscures spectrophotometric measurements; citrate/tartrate forms a soluble, stable chelate with Fe(III), keeping it in solution.